Low density steels are the collective name for some Fe-Mn-Al-C alloys.  Whereas the density of iron is 7.87 g/cm3, increasing the content of manganese (7.43 g/cm3) and aluminium (2.71 g/cm3) results in a product with an overall density lower than that seen in traditional low carbon steels. Since there is not a large density difference between manganese and iron, this article focuses on the impact of aluminium.  There are other benefits aside from lightweighting associated with increased manganese, and these are covered in our section on medium-manganese steels and twinning induced plasticity steels.

Low levels of aluminium, typically around 0.04%, are used to deoxidize most continuously cast steels.  Higher levels, around 1% to 2%, may be found in some TRIP or 3rd Generation AHSS grades. Still higher levels are used in an emerging family of products intended to retain the strength and formability benefits of advanced steels while exploiting the weight reduction potential that lower density aluminium offers.

Even though aluminium has a Face Centered Cubic (FCC) crystal structure similar to austenite, aluminium is a ferrite stabilizer in Fe-Al alloys having aluminium content greater than 6%. With sufficient carbon and manganese, this may change back to an austenitic structure.

In general, there are three classifications of high-aluminium steels for automotive applications.  Ferritic alloys are mainly iron and aluminium.  Two-phase austenite-ferrite alloys use C and Mn to stabilize austenite. Primarily austenitic alloys have relatively high levels of C and Mn, and are sometimes referred to as TRIPLEX steels because these have small amounts of ferrite and intragranular nanometer-sized precipitation of an ordered carbide known as the kappa (k) phase. Detailed reviews of these steels are found in Citations S-122 and G-54.  

One studyZ-21 evaluated two automotive parts stamped from a conventional CR-330Y-590T-DP (DP600) steel as a reference, and compared those parts made from an austenite-ferrite grade and a fully austenitic grade. The parts were a front side member needing energy absorption, and an A-Pillar where intrusion prevention is the critical parameter. For each part, the thickness of the low-density alloys were adapted to match the DP600 reference performances in terms of energy absorption and section forces. The results showed that the austenite-ferrite grade allowed for a 20% reduction in weight, while a 30% weight reduction was feasible with the fully austenitic grade. See Table 1 for details.Z-21 

Table 1: Calculated weight-saving potential of austenite-ferrite and austenitic lightweight steels relative to CR-330Y-590T-DP for a front side member and an A-Pillar. (Table based on Citation Z-21)
Phase Composition CR-330Y-590T-DP
(DP600; reference)
α ferrite + martensite
Iron-aluminium alloy with
Austenite-Ferrite Microstructure
Fe-Al: α + γ
Iron-aluminium alloy with
Austenite Microstructure
Fe-Al: γ
Chemistry (weight %) typical Fe- 0.2 C- 8.2 Mn- 7.4 Al Fe- 0.96 C- 25.8 Mn- 9.3 Al
YS (MPa) 330 min 646 812
TS (MPa) 590 min 812 1027
EL (%) 21 min 26 32
       
Front side member
Grade CR-330Y-590T-DP
(reference)
Fe-Al: α + γ Fe-Al: γ
Thickness FR/RR 1.7 mm / 2.1 mm 1.5 mm / 1.8 mm 1.3 mm / 1.7 mm
Total Mass per vehicle 5.88 kg 4.63 kg 3.99 kg
Mass savings per vehicle (reference) 1.25 kg 1.89 kg
Mass savings per vehicle  (reference) 21 % 32 %
       
A-Pillar
Grade CR-330Y-590T-DP
(reference)
Fe-Al: α + γ Fe-Al: γ
Thickness 1.6 mm 1.4 mm 1.25 mm
Total Mass per vehicle 6.11 kg 4.84 kg 4.12 kg
Mass savings per vehicle (reference) 1.27 kg 1.99 kg
Mass savings per vehicle (reference) 21 % 33 %

 

 

Another company states that low density steels are suitable for parts requiring high formability and weight reduction, such as body side reinforcement panels, rear crossmembers, and upper/lower covers of battery packs. These can be formed via cold stamping or roll forming. Some properties associated with these steels are found in Table 2.

Steel Grade Typical Mechanical Properties
Standard/Typical  Yield Strength (MPa)  Tensile Strength (MPa)  Total EL in 80mm (%)
CR-340/590-LD    Standard ≥ 340 ≥ 590 ≥ 21
Typical 443 618 29
CR-370/780-LD Standard ≥ 370 ≥ 780 ≥ 15
Typical 410 834 17
CR-420/780-LD Standard ≥ 420 ≥ 780 ≥ 13
Typical 521 834 22
CR-400/980-LD Standard ≥ 400 ≥ 980 ≥ 10
Typical 428 1038 15
Table 2: Properties of some low density steels.

 

 

Figures 1 and 2 show two part made from low density steels

Figure 1: Rear crossmember made from CR-340-590-LD low density steel.

Figure 1: Rear crossmember made from CR-340-590-LD low density steel.

 

Figure 2: Side Reinforcement Panels made from CR-340-590-LD low density steel.

Figure 2: Side Reinforcement Panels made from CR-340-590-LD low density steel.

 

 

Challenge with Galvanizing Low Density Steels

The external oxidation of aluminium prevents good wettability of zinc during hot dip galvanizing. This is a similar issue in 3rd Generation AHSS grades that use higher levels of aluminium. 

Increasing the dew point of the annealing furnace atmosphere from -50 °C to -10 °C promotes internal rather than external oxidation, and therefore is a viable strategy to improve galvanizability of low density steels.J-28 

 

Talk Like a Metallurgist

Talk Like a Metallurgist

Every industry has its own jargon. In certain settings, these words might be necessary – you wouldn’t want a cardiologist talking to a gastroenterologist about boo-boos and upset tummies. But when these professionals talk with their patients, it’s sometimes necessary for them to use much simpler words. That is, assuming the goal is to actually communicate the issues and concerns.

The steel industry is no different. We use words that have precise meanings in our daily discussions, and we forget that many people we work with don’t have exposure to the terminology that we are accustomed to using. What follows is a brief tour of the words and phrases you are likely to hear when speaking with your metallurgical representative.

Let’s start with the most common word: steel. Simply, steel is just an alloy of iron with up to about 2% carbon. Of course, other elements are in the composition. These fall into two categories: those intentionally added to improve one or more properties (called alloying elements), and those remaining from the steelmaking process that are too costly to remove relative to the benefit the removal would provide (called residual elements). High residuals are usually bad, typically because they lower ductility. But remember high is a relative term. The value may be higher than the standard to which you ordered (which is a cause for rejection), or just higher than what you’ve received in the past. If they are within the tolerance allowed within the standard, the product should still meet your strength and ductility requirements.

I’ve worked with metal formers who believe “steel is steel” and that all grades should behave the same way. According to the World Steel Association, there are more than 3,500 different grades of steel, each with unique properties and characteristics, 75% of which were developed in the past 20 years. Certainly, not all of these are sheet steels, but even within this category, there are sizable numbers. When it comes to just advanced high-strength sheet steels, more than 60 unique grades are available today.

The most common sheet steel grade is routinely called mild steel. Mild steels are low-carbon steels with no alloying elements added for substantial strengthening, and for that reason, they are characterized by relatively lower yield strength. However, there is no single grade or chemistry that meets this definition. Grade definitions require the steelmaker to meet certain chemistry or property limits. These grades are ordered to a standard usually written by the steel producer, a pertinent industry society (like ASTM, Euronorm, or JFS), or the end-user OEM. What is generally thought of as mild steel has chemistry, strength, and ductility overlapping many defined grades. Steel users should order to standards that define and constrain important properties like strength and ductility.

If you hang out with enough metallurgists, you are bound to hear passionate discussions about the iron-carbon phase diagram. (Why you are hanging around metallurgists is another topic entirely.) Before explaining the purpose of a phase diagram, it’s important to understand that a phase is a region of a material that is physically distinct, chemically uniform, and can be seen as different from the rest of the material. Ice and water are two phases that exist in my beverage. You’ll find a chocolate chip phase in my vanilla ice cream. And you’ll find ferrite in my steel – tasty! The properties of each of these change if you increase temperature (converting H2O from a solid to a liquid and eventually a gas) or if you add more alloying elements (chocolate chips or carbon). If you add a lot of that alloying element, you can get something entirely different like ripple or pearlite.

A phase diagram is a graphical representation of composition on the horizontal axis and temperature on the vertical axis. Two important phase diagrams are shown below. The far-left side of each represents 100% vanilla or 100% iron. Different phases exist as the temperature increases, or as the product is alloyed with increasing amounts of either chocolate or carbon.

 

Vanilla Chocolate Phase Diagram

Figure 1: Vanilla-Chocolate Phase Diagram A-77

 

Iron Carbon Phase Diagram

     Figure 2: Iron Carbon Phase DiagramA-78

 

Atoms arrange themselves in three-dimensional patterns called lattices. Think about billiard balls in multiple layers. The balls can be one layer directly above the prior one, or they can be shifted and rest in the crevice formed by adjacent balls in the layer below. The balls are all the same material, but the gap size changes with different arrangements. This is what happens with steel. At lower temperatures, only up to 0.02% carbon fits in the gap. This orientation is called ferrite. At higher temperatures, a different atomic orientation is stable, which we call austenite. Up to 2% carbon can fit into this arrangement of atoms. For low-carbon steels under normal conditions, austenite cannot exist at room temperature – when the steel is slowly cooled, it changes from austenite to a combination of ferrite and a mixture of phases called pearlite. However, heating a certain chemistry to the austenitic zone followed by rapidly cooling just right bypasses the natural conversion to ferrite and pearlite, and creates a structure that contains austenite at room temperature. This leads to the term retained austenite, which is the phase that gives TRIP and 3rd Generation Steels excellent ductility. More on these later.

100% iron is very soft. As a matter of fact, 100% of any element is very soft. As an example, think about gold. 24-carat gold is pure gold. You might think that a wedding ring, as a symbol of long-lasting love and devotion, should be made from 100% gold. In reality, many gold bands are made from 12-carat gold, which is half gold and half impurities. (Showing your love by giving something 50% impure perhaps is not the best marketing approach.) Adding alloying elements to gold is done to improve certain characteristics, like strength, making the alloy appropriate for the applications it serves.

When we talk about ferrite at room temperature, that’s iron with no more than 80 parts per million carbon. That’s really close to pure iron, so when we hear the term ferrite, we should think of something that is really soft, low-strength, and very ductile.

If additional strength is needed, then more alloying elements must be used in addition to carbon. The next most cost-effective alloying element is manganese which produces higher-strength steels called carbon-manganese steels. These are substitutional solid solutions strengthened, where the atoms of manganese swap into where atoms of iron would otherwise go. These grades have limited ductility, especially at higher carbon and manganese contents, so they are used in structural applications that do not need a lot of formability and are therefore also called structural steels (SS). In the ASTM standard specification covering many sheet steels, ASTM A1008/A1008M, these grades are grouped in the SS category.

Around 1980, steelmakers rolled out a new approach to getting higher strength levels while minimizing the loss of elongation usually seen with higher strengths. They do this by strengthening the ferrite through the addition of very small quantities of titanium, niobium, and vanadium to form carbide and nitride precipitates. These microalloying additions are used in precipitation hardening of the ferrite to create High Strength Low Alloy (HSLA) steels.

Switching gears a bit to discuss something unrelated to sheet steel but a process with which we might be familiar: forged gears. We want forged gears to be hard and high strength. Typical production of gears involves heating up a steel alloy of certain chemistry, followed by rapid cooling (quenching) them faster than a critical cooling rate. The structure that’s produced is called martensite. If the quench rate is only a little too slow, a different phase called bainite can be produced. While martensite is the highest strength phase, it has limited elongation. Bainite is a little lower in strength but has higher elongation and toughness compared with martensite. Bainite shines in applications needing cut-edge ductility during stretch flanging.

Martensite wasn’t commonly found as a microstructural component during most of the history of automotive sheet steels due to the limited number of companies having an annealing line with appropriate quenching capabilities. This started to change around the turn of the millennium when newer annealing lines were installed with the ability to hold at a specific temperature which may be lower than the annealing temperature followed by quenching to another much lower temperature. This led to greater production of the first generation of Advanced High-Strength Steels (AHSS), including grades that have a microstructure of only martensite. 

Dual Phase steels are the most common AHSS. As you might guess, there are two phases in Dual-Phase steels. Ferrite and martensite are the two phases: ferrite is super-soft and comprises the majority of the microstructure, while martensite is super-hard and takes up 10% (590DP) to 40% (980DP) of the microstructure. The more martensite, the stronger the steel. Elongation is the ductility measured in a tensile test, and since most of the structure is ferrite, these steels have exceptional elongation for the strength level. However, there is a large hardness difference between ferrite and martensite, leading to crack initiation sites and resulting in poor cut-edge ductility during stretch flanging.

[A brief digression on testing. Tensile testing takes a standard sample shape, typically looking like a bone you might give a dog to chew on, and pulls it in tension from the edges. The test results include yield strength, tensile strength, and total elongation, commonly called the YTEs or TYEs based on the initials. More information comes out of the tensile test, covered elsewhere. However, the tensile test is usually not used to measure cut-edge ductility. Cut edge ductility is typically characterized by the hole expansion test, where a punched hole is expanded with a conical punch until a through-thickness crack forms.]

Ferrite-bainite steels have a combination of decent elongation (from the ferrite) and excellent cut-edge ductility (from the bainite). Yes, your assumption is correct that there are only two phases in these steels, with ferrite being about 85% of the microstructure. Due to the way these are produced, ferrite-bainite steels are available as hot-rolled products only. That’s in contrast with Complex Phase (CP) steels, which can be found either at hot-rolled or cold-rolled thicknesses.

Soft ferrite is the primary microstructural component in DP steels and the soon-to-be-discussed TRIP steels, which results in low yield strength and relatively high elongation. On the other hand, the primary microstructural components of complex phase steels are bainite and precipitation-strengthened ferrite, with martensite and retained austenite also present in lower amounts. Lacking soft ferrite, these steels have relatively high yield strength and low elongation as measured in a tensile test, but the bainite leads to exceptional cut-edge ductility as measured in a hole expansion test. Multi-phase steels are a related product. Some OEMs group CP and MP steels in the same category, while others say that CP steels are engineered to favor improved bendability and cut edge extension over tensile elongation at the same tensile strength and that MP steels target balancing the fracture resistance needed for better bendability and hole expansion with the necking resistance found with higher uniform elongation and n-value.

TRIP steels contain mostly ferrite surrounding islands of martensite, as well as some bainite and retained austenite. The amount of bainite is pretty low, so it doesn’t add much to the cut-edge ductility. But the magic is in the retained austenite. Austenite is a very ductile phase. What makes this a special phase is that as austenite-containing steels deform, the atoms rearrange and the austenite transforms into martensite, giving the steel enhanced ductility. (Jargon alert: Another word for ductility used by professionals is plasticity.) A quick review: this enhanced ductility comes from austenite transforming to martensite. In other words, these steels have Transformation Induced Plasticity (TRIP).

Wouldn’t it be great to have an alloy that was just austenite? We’d have a high-strength, high-ductility product. There are two types of steels that are in this category. First are austenitic stainless steels in the 3XX family, like SS304 and SS316. In these alloys, austenite is stable at room temperature, but these require approximately 18% chromium and 8% nickel. Next are TWIP steels. These may look like TRIP steels from how they are written, but these steels get their plasticity differently. TWIP steels deform by a mechanism known as twinning, so they are described as Twinning Induced Plasticity Steels (TWIP). Of course, there are no free lunches. To get fantastic formability properties, a lot of alloying is necessary. This drives up the steelmaking complexity and cost. The alloying elements also make welding much more challenging. TWIP steels are called second-generation advanced high-strength steels.

The 3rd Generation Advanced High-Strength Steels (3rd Gen AHSS or 3rd Gen) are made possible by another advance in annealing technology, allowing steelmakers to produce a refined microstructure. Nearly all 3rd Gen steels have retained austenite in the microstructure and therefore benefit from a high strength, high ductility combination. The latest annealing lines used to make these steels come equipped to not just hold and quench to defined temperatures but have reheating capability followed by another hold and quench to different temperature targets. This allows for the creation of an engineered balance and distribution of ferrite, bainite, martensite, and austenite in the microstructure.

The resultant tensile property ranges from 3rd Gen steels produced at different companies may be similar, but their methods of getting those properties are a function of chemistry and the capabilities and characteristics of the equipment used to produce them. A different chemistry approach may result in different weldability, for example, so users are encouraged to perform thorough due diligence before switching suppliers. The days of steel being simply a commodity are in the past as it relates to these highly engineered higher strength steels.

 

Final thought 1: What’s an MPa?

This note may have a global readership, but this answer is focused on the countries that haven’t embraced the metric system. Megapascals, abbreviated MPa, is a measure of strength, just like pounds per square inch (psi) or force per area. Like Celsius and Fahrenheit or inches and millimeters, we can convert between them easily enough. There are 1000 psi in a ksi, with k being the abbreviation for kilopounds. And there are 6.895 ksi in an MPa. Make your life easier and focus on a 7:1 difference. 100 ksi is about 700 MPa.

 

Final thought 2: What about Press Hardening Steels?

Press hardening steel for hot stamping is a separate topic with a lot of nuances. One of the biggest differences is how the properties develop. For cold stamping operations, the stamping company is responsible for creating the formed part from sheet metal supplied to the necessary strength. With press hardening steels, the stamping company creates both the shape and the strength. Different grades come from a combination of different chemistries from the steelmaker and different heating and cooling profiles at the stamping location. The chosen corrosion protection approach impacts the various options. Learn more at the Press Hardening Primer on this site.

 

Final thought 3: Don’t hesitate to ask questions.

If your metallurgical representative says something that you don’t understand, ask for clarification. Your suppliers want to be your valued partner for more than just a simple transaction. Quite likely, your met rep is passionate about their offerings and would love to talk about them. If you get a deeper understanding of what makes one product different from another, then you’ll be in a better position to weigh the benefits against the inevitable constraints, leading to an optimized material selection. Remember, communication is the key to success for all parties.

 

Thanks go to author Daniel J. Schaeffler, Ph.D., President, Engineering Quality Solutions, Inc.

Danny Schaeffler is the Metallurgy and Forming Technical Editor of the AHSS Applications Guidelines available from WorldAutoSteel.  He is founder and President of Engineering Quality Solutions (EQS).  Danny writes the monthly “Metal Matters” column for Metalforming Magazine, and provides seminars on sheet metal formability for the Precision Metalforming Association.  He has written for Stamping Journal and The Fabricator, and has lectured at FabTech.  Danny is passionate about training new and experienced employees at manufacturing companies about how sheet metal properties impact their forming success.

 

 

Welcome to the All New AHSS Application Guidelines!

Welcome to the All New AHSS Application Guidelines!

The leading source for technical best practices on the forming and joining of Advanced High-Strength Steels (AHSS) for vehicle manufacture is released today by WorldAutoSteel, the automotive group of the World Steel Association. The AHSS Application Guidelines Version 7.0 is now online at ahssinsights.org in a searchable database, allowing users to pinpoint information critical to successful use of these amazingly capable steels. WorldAutoSteel members make these Guidelines freely available for use to the world’s automotive community.

“More and more automakers are turning to AHSS to balance the needs for crashworthiness, lighter weight and lower emissions, while still manufacturing cars that are affordable,” says George Coates, Technical Director, WorldAutoSteel. “The AHSS Application Guidelines provides critical knowledge that will help users adapt their manufacturing environment to these evolving steels and understand processes and technologies that lead to efficient vehicle structures.” AHSS constitute as much as 70 percent of the steel content in vehicle structures today, according to automaker reports.

New grades of steel that are profiled in Version 7.0 show dramatically increased strength while achieving breakthrough formability, enabling applications and geometries that previously were not attainable.

“Steel’s low primary production emissions, now coupled with efficient fabrication methods, as well as a strong global recycling and reuse infrastructure all create a solid foundation upon which to pursue vehicle carbon neutrality,” notes Cees ten Broek, Director, WorldAutoSteel. “These Guidelines contain knowledge gleaned from global research and experience, including significant investment of our members who are the designers and manufacturers of these steels.”

Editors and Authors Dr. Daniel Schaeffler, President Engineering Quality Solutions, Inc., for Metallurgy and Forming, and Menachem Kimchi, M.Sc., Assistant Professor – Practice, Materials Science and Engineering, Ohio State University, have drawn from the insights of WorldAutoSteel members companies, automotive OEMs and suppliers, and leading steel researchers and application experts. Together with their own research and field experience, the technical team have refreshed existing data and added a wealth of new information in this updated version.

The new database includes a host of new resources for automotive engineers, design and manufacturing personnel and students of automotive manufacturing, including:

  • Hundreds of pages of searchable articles that include nearly 1,000 citations of original technical research papers, providing a rich library for study.
  • Search tools and related posts fueled by thousands of industry-specific keywords that enable users to drill down to the information they need.
  • Information on the metallurgy and mechanics of AHSS grades.
  • An explanation of 3rd Gen AHSS and what makes these grades unique.
  • A primer on Press Hardened Steels, one of the most popular AHSS grades in today’s automotive structures.
  • Summaries of new research in resistance spot welding for joining AHSS of multiple grades and thicknesses.
  • New information on modelling resistance spot welding.
  • An expanded solid state welding section.
  • New information on RSW joining of dissimilar steels as well as dissimilar materials.
  • Articles written by subject-matter experts and product manufacturers.
  • Integration of the popular AHSS Insights technical blog.

The new online format enables consistent annual updates as new mastery of AHSS’s unique microstructures is gained, new technology and grades are developed, and data is gathered.  Be sure to subscribe to receive regular updates and blogs that represent a world of experience as the database evolves.

You’re right where you need to be to start exploring the database.  Click Tutorials from the top menu to get a tour on how the site works so you can make the best of your experience.  Come back often–we’re available 24/7 anywhere in the world, no download needed!

Metallurgy

Metallurgy

Metallurgy

The possibilities of combining iron with other elements and arranging them in novel ways are unparalleled and vast, which is why and how steel keeps reinventing itself from the mild automotive steels of the mid-20th Century to 3rd Generation Advanced High-Strength Steels today.

This section of the Guidelines provides a metallurgical look at the many steel types that make up automotive sheet steels.  But it is in no wise conclusive since the potential for new grades and attributes is still strong and will be well into the future. As an example, the UltraLight Steel Auto Body program, the first global steel industry automotive demonstration of High-Strength Steels (HSS) in vehicle applications, drew from a list of 11 HSS grades to manufacture its lightweight body structure. The Steel E-Motive program, the sixth steel industry demonstration, includes a portfolio of over 60 HSS and Advanced High-Strength Steel grades to design its optimized Mobility as a Service vehicle concepts.  Browse the Steel Grades page to review the family of automotive sheet steels.