3rd Generation Steels

3rd Generation Steels

 

First Generation Advanced High-Strength Steels (AHSS) are based on a ferrite matrix for baseline ductility, with varying amounts of other microstructural components like martensite, bainite, and retained austenite providing strength and additional ductility. These grades have enhanced global formability compared with conventional high strength steels at the same strength level. However, local formability challenges may arise in some applications due to wide hardness differences between the microstructural components.

The Second Generation AHSS grades have essentially a fully austenitic microstructure and rely on a twinning deformation mechanism for strength and ductility. Austenitic stainless steels have similar characteristics, so they are sometimes grouped in this category as well. 2nd Gen AHSS grades are typically higher-cost grades due to the complex mill processing to produce them as well as being highly alloyed, the latter of which leads to welding challenges.

Third Generation (or 3rd Gen) AHSS are multi-phase steels engineered to develop enhanced formability as measured in tensile, sheared edge, and/or bending tests. Typically, these steels rely on retained austenite in a bainite or martensite matrix and potentially some amount of ferrite and/or precipitates, all in specific proportions and distributions, to develop these enhanced properties.

Individual automakers may have proprietary definitions of 3rd Gen AHSS grades containing minimum levels of strength and ductility, or specific balances of microstructural components. However, such globally accepted standards do not exist. Prior to 2010, one steelmaker had limited production runs of a product reaching 18% elongation at 1000 MPa tensile strength. Starting around 2010, several international consortia formed with the hopes of achieving the next-level properties associated with 3rd Gen steels in a production environment. One effortU-11, S-95 targeted the development of two products: a high strength grade having 25% elongation and 1500 MPa tensile strength and a high ductility grade targeting 30% elongation at 1200 MPa tensile strength. The “exceptional-strength/high-ductility” steel achieved 1538 MPa tensile strength and 19% elongation with a 3% manganese steel processed with a QP cycle. The 1200 MPa target of the “exceptional-ductility/high-strength” was met with a 10% Mn alloy, and exceeded the ductility target by achieving 37% elongation. Another effort based in EuropeR-22 produced many alloys with the QP process, including one which reached 1943 MPa tensile strength with 8% elongation. Higher ductility was possible, at the expense of lower strength.

3rd Gen steels have improved ductility in cold forming operations compared with other steels at the same strength level. As such, they may offer a cold forming alternative to press hardening steels in some applications. Also, while 3rd Gen steels are intended for cold forming, some are appropriate for the hot stamping process.

Like all steel products, 3rd Gen properties are a function of the chemistry and mill processing conditions. There is no one unique way to reach the properties associated with 3rd Gen steels – steelmakers use their available production equipment with different characteristics, constraints, and control capabilities. Even when attempting to meet the same OEM specification, steelmakers will take different routes to achieve those requirements. This may lead to each approved supplier having properties which fall into different portions of the allowable range. Manufacturers should use caution when switching between suppliers, since dies and processes tuned for one set of properties may not behave the same when switching to another set, even when both meet the OEM specification.

There are three general types of 3rd Gen steels currently available or under evaluation. All rely on the TRIP effect. Applying the QP process to the other grades below may create additional high-performance grades.

  • TRIP-Assisted Bainitic Ferrite (TBF) and Carbide-Free Bainite (CFB)
    • TRIP-Assisted Bainitic Ferrite (TBF) and Carbide-Free Bainite (CFB) are descriptions of essentially the same grade. Some organizations group Dual Phase – High Ductility (DP-HD, or DH) in with these. Their production approach leads to an ultra-fine bainitic ferrite grain size, resulting in higher strength. The austenite in the microstructure allows for a transformation induced plasticity effect leading to enhanced ductility.
  • Quenched and Partitioned Grades, Q&P or simply QP
    • Quenching and Partitioning (Q&P) describes the processing route resulting in a structure containing martensite as well as significant amounts of retained austenite. The quenching temperature helps define the relative percentages of martensite and austenite while the partitioning temperature promotes an increased percentage of austenite stabile room temperature after cooling.
  • Medium Manganese Steels, Medium-Mn, or Med-Mn
    • Medium Manganese steels have a Mn content of approximately 3% to 12%, along with silicon, aluminum, and microalloying additions. This alloying approach allows for austenite to be stable at room temperature, leading to the TRIP Effect for enhanced ductility during stamping. These grades are not yet widely commercialized.

 

TRIP Assisted Grades, like TRIP-Assisted Bainitic Ferrite (TBF)

and Carbide-Free Bainite (CFB)

During the slow cooling of conventional steels, austenite transforms into a microstructure containing alternating regions of ferrite and cementite. Note that cementite is the name given to iron carbide with the composition Fe3C. At higher magnification, this microstructure looks like Mother-of-Pearl, leading to its name of pearlite.

Depending on the chemistry and thermal profile, rapid controlled cooling produces new microstructures which are not achievable with slow cooling, including martensite, austenite, and bainite. Bainite consists of regions of dislocation-rich (higher strength) ferrite separated by austenite, martensite, and/or cementite. These phases within bainite have relatively small hardness differences, leading to improved local formability compared with conventional dual phase or TRIP steels. Producing a fully-bainitic microstructure is challenging, so bainite is usually accompanied by other phases, resulting in ferrite-bainite steels or complex phase.

With an appropriate chemistry and use of specific thermal profiles capable of holding at specific temperatures and even reheating after quenching further reduces the size of these microstructural components, and essentially eliminates the production of the low-ductility cementite (iron carbide). Large “blocky” austenite, characteristic of 1st Generation TRIP steels, is minimized and instead thin fine submicron austenitic laths form (Figure 1).

Figure 1: On the left, the typical bainitic structure showing bainitic ferrite laths with interlath carbideS-96; On the right is the microstructure of TRIP Assisted Bainitic Ferrite / Carbide Free Bainite showing bainitic ferrite laths interwoven with thin films of untransformed retained austeniteC-31. ab is bainitic ferrite and y is retained austenite. Note the slightly different magnification.

Figure 1: On the left, the typical bainitic structure showing bainitic ferrite laths with interlath carbideS-96; On the right is the microstructure of TRIP Assisted Bainitic Ferrite / Carbide Free Bainite showing bainitic ferrite laths interwoven with thin films of untransformed retained austenite.C-31  αb is bainitic ferrite and γ is retained austenite. Note the slightly different magnification.

 

The fine components result in higher strength, similar to fine grain size being associated with increased strength. Since the ferrite is higher strength than conventional bainite due to the fine component size and even greater dislocation density, the component hardness difference is further minimized, leading to additional improvements in local formability. The austenite promotes the TRIP effect, resulting in greater uniform elongation and enhanced global formability. Combined, these features result in calling this microstructure either TRIP Assisted Bainitic Ferrite (TBF) or Carbide Free Bainite (CFB). Some sources suggest this is the same product as “Dual Phase with High Ductility,” abbreviated as DP-HD or simply DH.H-18, A-70, R-23, B-58  TBF, CFB, DP-HD, and DH are used interchangeably.

Examples of parts made from DH steels are found in Figure 2.  The retained austenite in the microstructure improves the edge ductility and bendability, making these parts feasible.

Figure 2: Parts made from DH steels. Crossmember component (CR330/590DH, top image), Seat crossmember (CR440/780DH, middle image), and Crossmember Front Floor (CR550/980DH, bottom image).

Figure 2: Parts made from DH steels. Crossmember component (CR330/590DH, top image), Seat crossmember (CR440/780DH, middle image), and Crossmember Front Floor (CR550/980DH, bottom image).

 

One potential processing route (Figure 3) may involve intercritical annealing in the two-phase austenite+ferrite region, cooling slightly to promote ferrite formation (1→2), and then quenching (2→3) to a temperature below the start of bainite formation (Bs) while remaining above the Ms temperature, the start of martensitic transformation. Once the targeted amount of bainite has formed in an isothermal overaging step (3→4), the steel is then quenched to room temperature (4→5).

Figure 2: Potential thermal cycle to produce TRIP assisted Bainitic Ferrite (Carbide-Free Bainite).

Figure 3: Potential thermal cycle to produce TRIP assisted Bainitic Ferrite (Carbide-Free Bainite).

 

These steels are characterized by a good balance of strength and global formability (as measured by high TSxEL, uniform elongation, and total elongation combined with low YS/TS) against local formability (as measured by bend angle and hole expansion ratio).C-31  A YS/TS ratio of approximately 0.7, similar to DP steels, is a characteristic of these grades.H-59, C-31

These steels exhibit a significant bake hardening response. One study found a BH kick of over 200 MPa after a 4% prestrain and a bake cycle of 30 minutes at 200 °C. The total hardening response (strain hardening plus bake hardening) was almost 800 MPa.T-41 However, in production, this paint bake cycle is not likely to be practical due to paint over curing and the preference for faster cycle times. A different study evaluated TBF700Y/1050T and found after 15 minutes at 195 °C, samples prestrained to 4.5% had a BH kick of 150 MPa, with a total hardening response in excess of 350 MPa.B-60

Challenges exist when producing these grades with a galvanized or galvannealed coating. The relatively higher silicon content needed to suppress carbide formation may lead to difficulties galvanizing and with galvanized surface quality. Replacing silicon with aluminum helps with the coating issues, but makes the thermal cycle more complex. The chosen thermal cycle needs to be appropriate for the selected chemistry and targeted properties, and constrained by the capabilities of the existing mill equipment. Descriptions of the capabilities of equipment used in the production of cold rolled and galvanized AHSS are found elsewhere.K-43, B-59

The 2013 Infiniti Q50 is one of the earliest production applications for TBF 1180, where it formed 4% of the Body-In-White mass. Applications included A- and B-pillar reinforcements, sill reinforcements, and roof rail and side reinforcements. Adjusted welding techniques resulted in the same stress concentration as seen when welding mild steels.I-22, K-44  The same grade applied on the 2015 Nissan Murano in the A-Pillar Inner and reinforcements allowed numerous components to be downgauged from 1.6 mm to 1.2 mm compared with the prior version.C-32 1180TBF represented over 6% of the mass of the 2016 Nissan Maxima body-in-white, primarily applied in the A- and B-Pillar Reinforcements. Typically, 1.4 mm thick 980 grade steel was downgauged to 1.2 mm.C-33

A sample of commercially available TBF1180 was shown to have 946 MPa yield strength, 1222 MPa tensile strength, 18% elongation (JIS sample) , with a 40% hole expansion ratioM-54, which is consistent with the minimum properties listed by one automotive OEM: YS: 850 MPa minimum, TS: 1180 MPa minimum, elongation: 14% JIS minimum, and 30% minimum hole expansion ratio.F-36  Stretch formability as tested using a dome height evaluation was shown to be comparable to a conventional DP980 product, with deep drawability characterized by forming height in a cup draw test being superior to both conventional DP980 and DP1180.

Stress-strain curves of TBF700Y/1050T are found in the literature and presented in Figure 4 for reference. Note that these are random samples from a commercially available product tested at different laboratories, and therefore may not be representative of all products of this grade.

Figure 3: Stress strain curves of commercially available TBF 700Y/1050T. A) YS=775 MPa, TS = 1235 MPa, EL = 10%G-44; B) YS=751 MPa, TS = 1035 MPa, EL = 17%. Also shown is the pre-strain and bake hardening response for 1.0 mm thick blanks, tested after a 20 minute dwell time in a 170°C furnace.B-60

Figure 4: Stress strain curves of commercially available TBF 700Y/1050T. A) YS=775 MPa, TS = 1235 MPa, EL = 10%G-44; B) YS=751 MPa, TS = 1035 MPa, EL = 17%. Also shown is the pre-strain and bake hardening response for 1.0 mm thick blanks, tested after a 20 minute dwell time in a 170 °C furnace.B-60

 

The 2018 Infiniti QX50 SUV is an example of a vehicle believed to have TBF980 in the body structure.I-23  The product shown is called SHF980, and has a microstructure of approximately 50% ferrite, approximately 10% retained austenite, with the remainder as martensite/bainite, which is consistent with expectations for a TBF product. The thermal processing route to achieve this microstructural balance is consistent with a Quenching & Partitioning process (Figure 5). Both SHF980 and the reference DP980 are shown to have 660 MPa yield strength and 1000 MPa tensile strength. However, where DP980 has 15% elongation, SHF980 has 23% elongation. In addition, SHF980 is capable of 10% greater energy absorption over DP980 at the same thickness.I-23

Figure 4: Production and properties of SHF980, possessing a TBF microstructure.I-23

Figure 5: Production and properties of SHF980, possessing a TBF microstructure.I-23

 

The highest strength TBF grade commercially available has 1,470MPa minimum tensile strength. Properties in Table 1 are compared with DP1470.

Table 1: Tensile properties of 1.2mm steels with 1470 MPa minimum tensile strength.M-55

Table 1: Tensile properties of 1.2mm steels with 1470 MPa minimum tensile strength.M-55

 

Case Study: Production Application Where 3rd Gen Steels

Reduced Weight and Improved Performance

Toyota Motor Europe designed a part requiring a minimum tensile strength of 980 MPa, but when stamped using a conventional AHSS grade, experienced both global formability (necking) failures and local formability (sheared edge) failures (Figure 6). In the search for a grade which blended the high elongation of dual phase grades and the high hole expansion of complex phase grades, Toyota chose TBF980, a TRIP-assisted bainitic ferrite grade with the same yield and tensile strength of a conventional 980 grade but with improved elongation of approximately 14% and hole expansion of approximately 65%.A-1

Also reported were grade and design changes in a production vehicle where the strength of TBF980 allows for a 20% thickness reduction over the prior model. The improved formability of TBF980 facilitated a reduction in packaging space of the component, with the new design being 6% narrower and 20% shorter.  Combined, these improvements reduced the vehicle weight by 1 kg.A-1

Figure 5: 980 MPa part with global and local formability failures.  Converting the steel to TBF980 eliminated both types of splits.  Image adapted from Citation A-1.

Figure 6: 980 MPa part with global and local formability failures.  Converting the steel to TBF980 eliminated both types of splits.  Image adapted from Citation A-1.

 

Quenched and Partitioned Grades, Q&P or simply QP

Quenching and partitioning (Q&P, or QP) describes a multi-step heat treatment which produces high tensile strength, high global ductility (total elongation) and high local ductility (hole expansion and bendability), compared with other similar strength steels. The QP process was first explained in 2003 by Speer et al.S-97, S-98, S-99

Among the unique aspects of the required thermal cycle is that after the first quench from the fully austenitized or intercritical annealing temperature, the steel may be reheated to a higher temperature, and then quenched to room temperature.

Figure 7 provides a general overview of the QP thermal cycle. After austenitization in either the single phase austenite region or the two-phase ferrite+austentite (intercritical annealing), the steel is quenched to a temperature below the start of martensitic transformation (Ms) but above the Mf (temperature at which all austenite has transformed to martensite), as indicated by segment 1→2. In the two-step QP process, the temperature is raised above Ms, shown in segment 2→3. No temperature increase is seen in the one-step QP process, meaning 2=3. Then the steel is held at this partitioning temperature for the appropriate time to generate the targeted microstructure and properties, segment 3→4. Once reached, the steel is quenched again (4→5), this time to a temperature below Mf, the temperature below which all transformation to martensite has occurred.

Figure 5: Thermal cycle for the Quenching and Partitioning Process.

Figure 7: Thermal cycle for the Quenching and Partitioning Process.

 

The QP microstructure contains martensite and austenite. Ferrite is also present if intercritical annealing in the two-phase region is employed rather than in the single-phase austenitic region. The first quench forms a controlled volume fraction of martensite. With a QP chemistry containing C between 0.15 and 0.4%, Mn between 1.5 and 2.5%,and (Al + Si) around 1.5 wt.%, the quenching temperature usually lies in the range 200 to 350 °C.S-100  After raising to the partitioning temperature typically between 300 to 500 °CS-100, an isothermal hold allows carbon from the carbon-supersaturated martensite to diffuse into the untransformed austenite. This enriches the austenite with carbon while similarly depleting the martensite. The carbon enriched austenite increases its room temperature stability. Since the partitioning temperature above that required for martensite formation, some of the martensite transforms to tempered martensite. Tempered martensite provides high strength with more ductility than untempered martensite. After the partitioning step, the final quench results in the formation of fresh martensite.

When stamping parts from this steel, the austenite transforms to newly formed martensite through the TRIP effect, enhancing the ductility and strength. Adjusting the chemistry, quenching temperature, partitioning temperature, and partitioning time affects the amount, morphology, and stability of the retained austenite, leading to a wide range of potential properties.D-32  The microstructure of commercial Q&P steels is composed of martensite (50–80%) formed during quenching, ferrite (20–40%) formed as austenite slowly cools, and dispersed retained austenite (5–10%) stabilized by carbon enrichment during partitioning. Higher strength QP steels will have reduced amounts of ferrite.W-35 This is mostly consistent with a study highlighting commercially produced QP980 and QP1180 which showed that both products have approximately 10-12% retained austenite, with QP980 containing 56% ferrite / 32% martensite and QP1180 containing 21% ferrite / 69% martensite.W-36

Common alloying additions for strengthening include manganese (Mn) and Silicon (Si), at levels of more than 2.2% and 1.5%, respectively, in QP steels.  During annealing, both elements move from the bulk substrate to the strip surface, and oxidize in the annealing atmosphere.  These surface oxides lead to poor wettability of both the phosphating solution and molten Zn on the steel surface, leading to surface defects.S-120, S-121 

Addressing these concerns means controlling the selective surface oxidation. One approach used is tuning the dew point of the annealing furnace atmosphere by converting the external oxidation into internal oxidation.Z-19

There is no standard processing route with defined chemistry and temperatures. The complex thermal cycle needs to be appropriate for the selected chemistry and targeted properties, and constrained by the capabilities of the existing mill equipment. Citation K-43 presents descriptions of the equipment and capabilities used at one location. Process variants exist, such as a one-step approach using the same temperature for the initial quench and the partitioning.S-98  Other modifications allow for production of a Carbide-Free Bainitic structure during the first quench, improving the damage resistance due to additional strain-hardening capacity within the local plasticity deformation zone near the tips of micro-cracks.G-45

The Q&P process is applicable to other products as well, including stainless steelsM-56, M-57, S-101 and Press Hardening Steels.A-71, A-72, X-1  A one-step Q&P approach was applied to a laser welded blank with 22MnB5 and TRIP components, resulting in tailored properties to improve the intrusion resistance and energy-absorption capabilities in the pertinent regions.K-46

Complex phase steels with High Ductility (CP-HD, or CH) have similar microstructural constituents, along with bainite. Although CH steels reach high hole expansion values, they do not have the elongation levels typically associated with QP steels. Still, some sources equate CH and QP steels.H-18

Two levels of Quenched & Partitioned steels are in global production, 980 MPa and 1180 MPa. The enhanced properties of QP steels offer benefits over similar-strength steels of other microstructures. Compared against Dual Phase steel with similar yield and tensile strength, a Quenched & Partitioned steel showed higher uniform elongation, total elongation, work hardening index, and FLC0, highlighted in Table 2 and Figure 8.C-34  A different production supplier of QP980 reports similar strength and elongation properties, with a targeted 23% hole expansion ratio.G-46

Table 2: Tensile properties of production DP980 and QP980.C-34

Table 2: Tensile properties of production DP980 and QP980.C-34

 

Figure 6: Comparison of Forming Limit Curves of production DP980 and QP980.C-34

Figure 8: Comparison of Forming Limit Curves of production DP980 and QP980.C-34

 

QP980 is seeing expanded use in automotive production. The 2016 Chevrolet Sail from SAIC-GM represented the first application at General Motors.H-60  The 2021 Ford Bronco uses hot dip galvanized QP980 in five components of the front and rear floor assemblies.S-102  Sixty percent of the body structure of the 2021 Jeep Grand Cherokee L is made from AHSS, with some parts stamped from 3rd Gen steels.F-37

Table 3 contains typical mechanical property ranges for industrially produced QP980 and QP1180.W-35  A typical strain–stress curve of QP980 is shown in Figure 9.

Table 3: Typical mechanical property ranges for industrially produced QP980 and QP1180.W-35

Table 3: Typical mechanical property ranges for industrially produced QP980 and QP1180.W-35

 

Figure 7: Stress-strain curve of industrially produced QP980.W-35

Figure 9: Stress-strain curve of industrially produced QP980.W-35

 

Of course, there are additional characteristics beyond strength and elongation that impact successful use in manufactured products. Typical forming-limit curves for cold rolled QP980, DP780, and DP 980 steels are shown in Figure 10, highlighting that the formability of QP980 is comparable to that of DP780.

Figure 8: Forming-limit curves for 1 mm thick Q&P 980, DP 780, and DP 980.W-35

Figure 10: Forming-limit curves for 1 mm thick Q&P 980, DP 780, and DP 980.W-35

 

Figure 11 contains the results of high strain rate tensile testing, confirming that QP980 has positive strain rate sensitivity and therefore has the potential for improved crash energy absorption.

Figure 9: True stress-strain curves for QP980 generated at different strain rates.W-35

Figure 11: True stress-strain curves for QP980 generated at different strain rates.W-35

 

Sheared-edge ductility is also a concern in AHSS grades. Hole expansion of QP1180, QP980, and DP980 is compared in Figure 12, with similar results seen in QP980 and DP980. QP1180 had the highest hole expansion, possibly because of its microstructure containing components of relatively uniform hardness.

Figure 10: Hole expansion of QP1180, QP980, and DP980, generated from either punched or machined holes.W-35 

Figure 12: Hole expansion of QP1180, QP980, and DP980, generated from either punched or machined holes.W-35

 

The bending under tension test was used to determine the critical R/t value below which the risk for shear fracture increases. These experiments showed that critical R/t values of QP980 were close to those of other steels having 600 MPa tensile strength.W-35

Similar springback was observed in QP980 and DP980 when a 5 mm radius was used in the bending-under-tension test, with QP980 exhibiting less springback when a 12.7 radius die was used instead.W-35

General Motors provided stress-strain curves for production QP700/1180 tested at different strain rates (Figure 13), showing increases in strength and ductility as strain rates increase.H-60

Figure 11: Engineering stress-strain curves for QP700Y/1180T at different strain rates.H-60

Figure 13: Engineering stress-strain curves for QP700Y/1180T at different strain rates.H-60

 

The stress-strain curves of some advanced steels are compared in Figure 14.  The ductility benefit of Quenched and Partitioned steels is seen in the greater elongation.

 
Figure 14: Stress strain curves of four advanced steels.

Figure 14: Stress strain curves of four advanced steels.

 

A recent conference highlighted several applications (Figure 15) where thinner gauge QP980 replaced DP590 in General Motors vehicles.W-37

Figure 15: Replacing DP590 with QP980 allows for downgauging.W-37

Figure 15: Replacing DP590 with QP980 allows for downgauging.W-37

 

The same presentationW-37 showed the example of QP980 replacing press hardening steels in B-pillar reinforcements and door anti-intrusion beams in a First Auto Works vehicle, Figure 16.

Figure 16: QP980 may replace press hardening steels in some safety applications.W-37

Figure 16: QP980 may replace press hardening steels in some safety applications.W-37

 

Development work continues to extend the upper limits of strength.  A grade referred to as S1500 has a martensitic matrix with retained austenite dispersed throughout. It is similar to QP980, but with a higher martensite content and a lower retained austenite content than QP980. S1500 has yield and tensile strength comparable to MS1500, but with substantially higher elongation to fracture (a measure of global ductility) and fracture strain within a very small region (a measure of local ductility).J-27

Table 4 shows the properties of these three grades, and a comparison of stress-strain curves can be found in Figure 17.

Table 4: Properties of Three Advanced High Strength Steels. Table based on Citation J-27.

Steel
Type
Thickness
(mm)
YS
(MPa)
TS
(MPa)
Fracture
Elongation (%)
n r0 r45 r90 Fracture strain:
0.5 mm x 0.5 mm
S1500 1.5 1363 1503 12.90 0.04 0.79 0.83 0.80 0.520
MS1500 1.2 1311 1502 5.76 0.04 — — — 0.357
QP980 1.4 764 1085 19.70 0.16 0.85 0.91 1.03 0.441

 

Figure 17. Stress-Strain curves of MS1500, QP980, and S1500.J-27

Figure 17. Stress-Strain curves of MS1500, QP980, and S1500.J-27

 

The phase transformations occurring in the two grades containing retained austenite, combined with the impact on instantaneous n-value, help explain the difference in forming behavior with the grade that is 100% martensite, Figure 18.

Figure 18: Hardening curves and instantaneous n-values of S1500, MS1500, and QP980. J-27

Figure 18: Hardening curves and instantaneous n-values of S1500, MS1500, and QP980.J-27

 

Without any phase transformation in MS1500 (green curves in Figure 18), the instantaneous n-value peaks and drops down. Limited strengthening in this grade leads to relatively low elongation at break.

The relatively high n-value associated with QP980 (red curves in Figure 18) indicates a superior ability to distribute strains over a wider region than the other two grades, and is associated with substantial strengthening with strain (work hardening).  The greater amount of retained austenite leads to the TRIP effect occurring early in the application of strain, leading to a rise in n-value in these early stages. QP980 continues to maintain a high n-value in the later stage of uniform deformation, leading to high elongation at break.

The S1500 (black curves in Figure 18) has a microstructure of nearly 90% martensite, so it is not surprising that during the initial application of strain, the behavior is similar to that seen in MS1500: The martensite deforms first. After an early peak in instantaneous n-value, it decreases rapidly.  However, as application of strain continues, n-value begins to rise in the S1500 grade. This occurs because the retained austenite in the microstructure undergoes the TRIP effect and produces fresh strain-induced martensite.

MS1500 does not increase in the later stage of uniform strain. These differences may be correlated with the volume fraction of the retained austenite.

 

Enhancing the TRIP Effect in QP Steels

The strength-ductility balance of quenched and partitioned steels results from the TRIP effect.  The magnitude of the TRIP effect is controlled by the amount of retained austenite in the microstructure.  A thermal cycle known as Q&Q-P (pre-quenching followed by quenching & partitioning) can increase the volume fraction of retained austenite, and therefore improves the mechanical properties of these alloys.Z-17

The pre-quench process consists of austenitizing followed by quenching to room temperature.  This results in a fine martensitic microstructure. This starting point leads to an increased density of austenite grain nucleation sites during subsequent annealing, producing fine austenitic grains. The second quench of the Q&Q-P process, or the initial quench of the Q-P process, is not taken to room temperature, but instead to a temperature between the martensite-start (Ms) and martensite-finish (Mf) temperatures. In the partitioning step, these quenched sheets are held either at or above this initial quenching temperature in order to enrich the untransformed austenite by carbon diffusion from supersaturated martensite.

A reduction in the austenite grain size from the pre-quench step increases the austenite stability by lowering the starting temperature for martensitic transformation, thereby suppressing the martensite transformation, meaning that the TRIP effect continues to enhance ductility even at greater forming strains. Smaller austenite grain size results in increased strength, and increases the mechanical free energy required to transform into martensite.  

A schematic of the Q&Q-P and Q-P process is shown in Figure 19.

Figure 19: Schematic of the Q&Q-P (with prequench) and Q-P (Quenching & Partitioning) heat treatment cycles. Z-17

Figure 19: Schematic of the Q&Q-P (with prequench) and Q-P (Quenching & Partitioning) heat treatment cycles.Z-17

 

The time of partitioning influences properties due to the change in the volume fraction of retained austenite, as indicated in Table 5.  Even with the impact of the partitioning time, the pre-quench process results in a substantial increase in retained austenite.
 

Table 5: Volume fraction (%) of retained austenite as a function of partitioning time in the Q-P and Q&Q-P process. Z-17
  5 s 10 s 20 s 50 s 100 s 200 s
Q-P 13.9 11.6 11.3 10.5 12.1 11.2
Q&Q-P 19.3 19.9 22.5 20.4 20.4 21.6

 

The microstructure of Q-P samples consists of martensite and retained austenite, where the martensite deforms plastically in the early strain stage, leading to local stress concentration occurring at small strains. The retained austenite transforms in order to relieve the local stress concentration and is exhausted at these small strains.

In contrast, the Q&Q-P samples contain ferrite, which is the first to deform preferentially in the early strain stages.  This behavior, plus the higher volume fraction of retained austenite, allows the Q&Q-P samples to continue deforming by the TRIP effect at higher strains. Depending on the partitioning time, 1000 MPa tensile strength with elongation approaching 30% is achievable.Z-17

 

Medium Manganese Steels, Medium-Mn, or Med-Mn

Manganese has a lower density than iron, so using alloys with higher amounts of manganese truly creates lightweight products. 1st Generation steels typically contain no more than around 2% Mn. 2nd Generation TWIP steels have about 20% Mn. Lean medium-manganese (MedMn) steels typically use between 3% and 12% manganese along with silicon, aluminum, and microalloying additions.R-16, D-27, S-80, K-35  Aluminum in these steels further lowers the density.

No standard chemistry or processing route exists, but several studies use a thermal cycle similar to that seen with Q&P steels. This approach leads to a complex multiphase fine-grained microstructure. Compared with QP steels at the same strength levels, the higher manganese levels of Med-Mn steels promote greater amounts of retained austenite, and therefore greater ductility through the TRIP Effect. One study showed a combination of 1400 MPa tensile strength and a total elongation of 18%.S-103

One difference from the thermal cycle to produce QP steels used by some researchers to process Med-Mn steels is that after intercritical (two-phase) annealing, the quench is to room temperature rather than simply below Ms, the start of martensitic transformation.S-80 This is facilitated by the high levels of manganese, which adjusts the Mf below room temperature. Quenching a steel containing 0.25% C, 8.23% Mn, 1.87% Si, 0.05% Ni, and 0.24% Mo to room temperature and subsequently partitioning at 300 °C led to tensile strengths greater than 1800 MPa combined with total elongations of approximately 15%.S-80

In addition to lowering the Mf (martensite finish) level below room temperature, the manganese levels are sufficiently high enough that the coils after hot rolling may be either partially or fully martensitic. This phenomenon means that it may be possible to produce hot rolled Med-Mn steels.

Another production method called Austenite-Reverted Transformation (ART) annealing results in a large percentage of retained austenite in medium manganese steels. The fully or partially martensitic hot or cold rolled coil is heated to the single phase austenite region or the intercritical two phase austenite+ferrite region where the martensite reverts to austenite – hence the name of the process. The austenite nucleates on the former sites of fine martensitic features. This approach results in a final product with extremely fine features. During annealing, diffusion of both carbon and manganese occurs, which determines both the phase fraction and stability of the retained austenite. Processing of Fe–0.3C–11.5Mn–5.8Al resulted in a microstructure with 60% retained austenite.B-59

Multi-step thermal treatments are one approach to control the relative proportions of martensite, ferrite, and austenite. One example, termed “double-soaking” (DS), aims for substantial Mn-enrichment of austenite in a first soaking step followed by a second soaking step at a higher temperature which leads to a greater fraction of martensite in the final product. The brief second soak is long enough to allow the carbon to partition, but not long enough for manganese partitioning to occur, producing regions of higher and lower Mn within the austenite. The higher-Mn regions allow for greater amounts of austenite in the final product, while the lower-Mn regions transform to martensite, leading to TRIP-effect ductility and high strength.S-80, G-47 In an industrial environment, the initial soak may be done in a batch anneal furnace, with the brief second soak targeted for the time and temperature available in continuous annealing or galvanizing lines.

Still another production method proposed is known as Deforming and Partitioning (D&P). This route uses a warm rolling followed by cold rolling to generate an extremely high dislocation density. A subsequent partitioning treatment relieves the residual stresses from rolling and stabilizes the retained austenite via carbon enrichment. Figure 19 shows a representative Deforming and Partitioning thermal cycle. A D&P MedMn steel with a composition of 0.47C–10Mn–2Al–0.7V reached a yield strength of 2.2 GPa (2,200 MPa) and a uniform elongation of 16%.H-65

Figure 15: Representative Deforming and Partitioning (D&P) thermal cycle

Figure 19: Representative Deforming and Partitioning (D&P) thermal cycle.H-65

 

Medium-manganese steels with Mn contents between 3 wt.% and 10 wt.% have a microstructure consisting of an ultra-fine grained ferritic matrix (grain size < 1 μm) with up to 40 vol.% retained austenite.K-47  A chemistry of Fe-7.9Mn-0.14Si-0.05Al-0.07C resulted in 39% retained austenite with the processing route evaluated.Z-10

Properties are dependent on all aspects of the chosen chemistry and thermal cycle. With an appropriate approach, the steel may exhibit both a transformation-induced plasticity (TRIP) effect and a twinning-induced plasticity (TWIP) effect.

Studies indicate that Medium Manganese steels are also suitable for use in press hardening applications. A studyL-63 indicates that an alloy with 0.14 %C – 7.0 %Mn rivals conventional 22MnB5 PHS1500 in strength, but has more ductility. After hot forming and processing through a typical paint bake cycle, 22MnB5 exhibited a tensile strength of 1510 MPa, a uniform elongation of 4.6%, and a total elongation of 7.3%.  The MedMn steel showed values of 1565 MPa, 9.6% and 11.7% respectively, Figure 20.  These enhanced properties are suspected to be associated with the high volume fraction (15%) of retained austenite found in the Medium Manganese steels.

Figure 16: Engineering stress–strain curves of the medium-Mn martensitic steel and 22MnB5.

Figure 20: Engineering stress–strain curves of the medium-Mn martensitic steel and 22MnB5.L-63

 

Unlike TBF and QP steels, Medium-Manganese steels may exhibit discontinuous yielding, also known as yield point elongation or Lüders bands. Depending on chemistry and processing, these may extend beyond 5% engineering strain.

Medium manganese steels are not yet widely commercialized. They were the focus of an entire issue of a technical journal.M-58  The lead Editorial presents an overview of prior studies and highlights areas of interest.R-16

 

Consortia Activities on Hot Press Forming

Under the leadership of Tata Steel Nederland, the European Commission through the European Research Executive Agency has funded a multi-year study called WarP-AHSS, which stands for Warm Press-Formed Zinc-Coated Third Generation Advanced High Strength Steels with High Crash and Corrosion Resistance and Minimized Microcracking.

Many issues with the traditional hot forming of aluminum-silicon (AlSi) coated press hardening steels (PHS) austenitized at ~900 °C inspired the interest in this topic. First, the galvanic corrosion protection offered by zinc coated steels is generally superior to the barrier corrosion protection seen with AlSi coatings. However, by the time that zinc coated steels reach the ~900 °C necessary to achieve full austenitization, the coated layer of zinc has already melted and possibly also started to vaporize. Furthermore, any liquid zinc produced during blank reheating will seep into the austenite grain boundaries under forming load and create microcracks on the steel surface– known as liquid metal embrittlement (LME). The microcracks are initiation points for corrosion and can act as stress concentrators that weaken the component under load (particularly for surface dependent properties such as fatigue and bendability).

The WarP-AHSS project seeks to develop end-to-end processing of warm press-formed parts from zinc-coated Medium Manganese Steels. This project focuses on a process that lowers the hot-forming temperature sufficiently to preserve the integrity of the zinc coating while maintaining the steel’s ability to reach the targeted strength and ductility levels.

Two products are under development that will provide improved options to crash energy management strategies deployed by automakers:

  1. Intrusion-resistant steel such as those used for side-impact components like the upper portion of B-Pillars. This product is intended to have similar strength as conventionally processed press hardened steels (≥ 1500 MPa) but with improved total elongation (≥ 10%, compared to ≥ 6% found with conventional PHS).
  2. Energy-absorbing steel such as those used in components like front and rear longitudinal rails or the lower section of B-Pillars. Compared to the intrusion-resistant steel, these energy absorbing steels sacrifice some strength (≥ 1200 MPa) to achieve even higher total elongation (≥ 18%), reaching more than double of the energy-absorption capacity of the product (as measured by tensile strength x total elongation) compared to conventional PHS.

Reducing the blank reheating and forming temperatures compared with the conventional press hardening process also reduces the energy consumption per component produced, contributing to a lower carbon footprint. The lower temperatures, combined with use of zinc coating, also lead to reduced tool wear compared to the conventional process where the hard intermetallics formed due to use of AlSi coating and thermal stress on dies and tooling amplify the need for their maintenance or replacement. The WarP-AHSS process mitigates this thermal degradation, which extends tool life and reduces production line downtime.

Furthermore, resistance spot welding (RSW) of AlSi-coated automobile components is more complex than welding zinc-coated parts. The AlSi coating evolves into different layer structures as a function of the thermal profile during hot stamping. The chemistries of these intermetallic layers are different, with each having distinct electrical contact resistances. Insufficient process control may therefore result in spatter and porosity within the weld nugget.

Partners in the WarP-AHSS research project include a steelmaker, an automaker, a university, and three research institutions. The project was initiated in October 2023. Progress continues to be made, documented in several research papers, conference presentations and seminars, and is on track for completion by the project end date in 2027.

The European Research Executive Agency has funded another multi-year study, Sup3rForm, that seeks to optimize the production and use of both 3rd Generation Q&P and medium-Mn steels. The Sup3rForm consortium, coordinated by Eurecat Technology Centre, is made up of eight partners, including steelmakers, an automaker, tier suppliers, and universities. Sup3rForm runs from July 2023 through December 2026.

 

Back To Top

Carbon-Manganese (CMn)

Carbon-Manganese High Strength Steel

Carbon and manganese are the two most cost-effective alloying additions to increase strength.  While effective at strengthening, these additions reduce ductility and toughness, and make welding more challenging.

The practical usage of these grades typically limits the highest strength to no more than 280 MPa.  Adding enough carbon and manganese to achieve higher strength results in a product without sufficient ductility for challenging applications, low toughness, and welding difficulty. These products sometimes are referred to as structural steels, and achieve their strength from the mechanism of solid solution strengthening.

Until the commercialization of High Strength Low Alloy steels, the CMn approach was the only option for users to obtain a high strength sheet metal.

Some of the specifications describing uncoated cold rolled Carbon-Manganese (CMn) or structural steels are included below, with the grades typically listed in order of increasing minimum yield strength and ductility. Different specifications may exist which describe hot or cold rolled, uncoated or coated, or steels of different strengths. Many automakers have proprietary specifications which encompass their requirements.  Note that ASTM terminology is based on minimum yield strength, while JIS and JFS standards are based on minimum tensile strength.  Also note that JIS G3135 does not explicitly state that these grades must be supplied with a C-Mn chemistry.  An HSLA approach is satisfactory as long as the mechanical property criteria are satisfied.

  • ASTM A1008M, with the terms Grade 25 [170], Grade 30 [205], Grade 33 [230] Type 1, Grade 33 [230] Type 2, Grade 40 [275] Type 1, Grade 40 [275] Type 2, Grade 45 [310], Grade 50 [340], Grade 60 [410], Grade 70 [480], and Grade 80 [550] A-25
  • JIS G3135 with the terms SPFC340, SPFC370, SPFC390, SPFC440, SPFC490, SPFC540, and SPFC590 J-3
  • JFS A2001, with the terms JSC340W, JSC370W, JSC390W, and JSC440W J-23

 

 

3rd Generation Steels

Twinning Induced Plasticity

TWinning Induced Plasticity (TWIP) steels have the highest strength-ductility combination of any steel used in automotive applications, with tensile strength typically exceeding 1000 MPa and elongation typically greater than 50%.

TWIP steels are alloyed with 12% to 30% manganese that causes the steel to be fully austenitic even at room temperature. Other common alloying additions include up to 3% silicon, up to 3% aluminum, and up to 1% carbon. Secondary alloying additions include chromium, copper, nitrogen, niobium, titanium, and/or vanadium.D-29 The high alloying levels and substantially greater levels of strength and ductility place these into the 2nd Generation of Advanced High Strength Steels. Furthermore, due to the density of the major alloying additions relative to iron, TWIP steels have a density which is about 5% lower than most other steels.

Calling this type of steel TWIP originates from the characteristic deformation mode known as twinning. Deformation twins produced during sheet forming leads to microstructural refinement and high values of the instantaneous hardening rate (n-value). The resultant twin boundaries act like grain boundaries and strengthen the steel. On either side of a twin boundary, atoms are located in mirror image positions as indicated in the schematic microstructure shown in Figure 1. Figure 2 highlights the microstructure of TWIP steel after annealing and after deformation.

Figure 1: Schematic of TWIP steel microstructure.

Figure 1: Schematic of TWIP steel microstructure.

 

Figure 2: TWIP steel in the annealed condition (left) and after deformation (right) showing deformation twins. The number of deformation twins increases with increasing strain.K-42

Figure 2: TWIP steel in the annealed condition (left) and after deformation (right) showing deformation twins. The number of deformation twins increases with increasing strain.K-42

 

EDDS or Interstitial-Free or Ultra-Low Carbon steels are different descriptions for the most formable lower-strength steel. Possible test results for this grade are 150 MPa yield strength, 300 MPa tensile strength, 22% to 25% uniform elongation, and 45% to 50% total elongation. In contrast, test results on TWIP steels may show 500 MPa yield strength, 1000 MPa tensile strength, 55% uniform elongation, and 60% total elongation.

The stress-strain curves for these two grades are compared in Figure 3. The TWIP curves show the manifestation of Dynamic Strain Aging (DSA), also known as the PLC effect, with more details to follow.

Figure 3: Uniaxial tensile stress-strain curves for an interstitial-free (IF) extra-deep-drawing steel and an austenitic Fe-18%Mn-0.6%C-1.5%Al TWIP steel. Curves are presented both terms of engineering (s,e) and true (σ,ε) stresses and strains, respectively.D-30

Figure 3: Uniaxial tensile stress-strain curves for an interstitial-free (IF) extra-deep-drawing steel and an austenitic Fe-18%Mn-0.6%C-1.5%Al TWIP steel. Curves are presented both terms of engineering (s,e) and true (σ,ε) stresses and strains, respectively.D-30

 

Figure 4 compares the results of bulge testing ferritic interstitial-free (IF) steel and austenitic Fe-18%Mn-0.6%C-1.5%Al TWIP steel. The TWIP steel is still undamaged at a dome height that is 31% larger than the IF steel dome height at failure.D-30

Figure 4: Comparison of dome testing between EDDS and TWIP.D-30

Figure 4: Comparison of dome testing between EDDS and TWIP.D-30

 

Excellent stretch formability is associated with high n-values. Shown in Figure 5 is a plot showing how the instantaneous n-value changes with applied strain. N-value increases to a value of 0.45 at an approximate true (logarithmic) strain of 0.2 and then remains relatively constant until an approximate true strain of 0.3 before increasing again. The high and uniform n-value delays necking and minimizes strain peaks. Twins continue to form at higher strains, leading to finer microstructural features and continued increases in n-value at higher strains.

Figure 5: Instantaneous n-value changes with applied strain. TWIP steels have high and uniform n-value leading to excellent stretch formability.C-30

Figure 5: Instantaneous n-value changes with applied strain. TWIP steels have high and uniform n-value leading to excellent stretch formability.C-30

 

A microstructural deformation phenomenon known as the Portevin-LeChatelier (PLC) effect occurs when deforming some TWIP steels to higher strain levels. The PLC effect is known by several other names as well, including jerky flow, discontinuous yielding, and dynamic strain aging (DSA).

The severity varies with alloy, strain rate, and deformation temperature. Figure 6 shows how DSA affects the appearance of the stress strain curve of two TWIP alloys.D-29 The primary difference in the alloy design is the curves on the right are for steel containing 1.5% aluminum, with the curves on the left for a steel without aluminum. The addition of aluminum delays the serrated flow until higher levels of strain. Note that both alloys have negative strain rate sensitivity.

 

Figure 6: Influence of aluminum additions on serrated flow in Fe-18%Mn-0.6%C TWIP (Al-free on the left) and Fe-18%Mn-0.6%C-1.5% Al TWIP (Al-added on the right).D-29

Figure 6: Influence of aluminum additions on serrated flow in Fe-18%Mn-0.6%C TWIP (Al-free on the left) and Fe-18%Mn-0.6%C-1.5% Al TWIP (Al-added on the right).D-29

 

The primary macroscopic manifestations of the Portevin-LeChatelier (PLC) effect areD-29:

  • negative strain rate sensitivity.
  • stress-strain curve showing serrated or jerky flow, indicating non-uniform deformation. Strain localization takes place in propagating or static deformation bands.
  • the strain rate within a localized band is typically one order of magnitude larger, while that outside the band is one order of magnitude lower, than the applied strain rate.
  • limited post-uniform elongation, meaning uniform elongation is just below total elongation. Said another way, fracture occurs soon after necking initiation.

The PLC effect leads to relatively poor sheared edge expansion, as measured in a hole expansion test. Figure 7 on the left highlights the crack initiation site in a sample of highly formable EDDS-IF steel, showing the classic necking appearance with extensive thinning prior to fracture. In contrast, note the absence of necking in the TWIP steel shown in the right image in Figure 7.D-29

Figure 7: Sheared edge ductility comparison between IF (left) and TWIP (right) steel. TWIP steels lack the sheared edge expansion capability of IF steels. D-29

Figure 7: Sheared edge ductility comparison between IF (left) and TWIP (right) steel. TWIP steels lack the sheared edge expansion capability of IF steels.D-29

 

The stress-strain curves of several TWIP grades are compared in Figure 8.

Figure 8: Engineering stress-strain curve for several TWIP Grades.P-30

Figure 8: Engineering stress-strain curve for several TWIP Grades.P-18

 

Complex-shaped parts requiring energy absorption capability are among the candidates for TWIP steel application, Figure 9.

Figure 9: Potential TWIP Steel Applications.N-24

Figure 9: Potential TWIP Steel Applications.N-24

 

Early automotive applications included the bumper beam of the 2011 Fiat Nuova Panda (Figure 10), resulting in a 28% weight savings and 22% cost savingsN-24 over the prior model which used a combination of PHS and DP steels.D-31

Figure 10: Transitioning to a TWIP Bumper Beam Resulted in Weight and Cost Savings in the 2011 Fiat Nuova Panda. N-24, D-31

Figure 10: Transitioning to a TWIP Bumper Beam Resulted in Weight and Cost Savings in the 2011 Fiat Nuova Panda. N-24, D-31

 

In the 2014 Jeep Renegade BU/520, a welded blank combination of 1.3 mm and 1.8 mm TWIP 450/950 (Figure 11) replaced a two-piece aluminum component, aiding front end stability while reducing weight in a vehicle marketed for off-road applications.D-31

Figure 11: A TWIP welded blank improved performance and lowered weight in the 2014 Jeep Renegade BU/520.D-31

Figure 11: A TWIP welded blank improved performance and lowered weight in the 2014 Jeep Renegade BU/520.D-31

 

Also in 2014, the Renault EOLAB concept car where the A-Pillar Lower and the Sill Side Outer were stamped from TWIP 980 steel.R-21 By 2014, GM Daewoo used TWIP grades for A-Pillar Lowers and Front Side Members, and Hyundai used TWIP steel in 16 underbody parts. Ssangyong and Renault Samsung Motors used TWIP for Rear Side Members.I-20

Other applications include shock absorber housings, floor cross-members, wheel disks and rims, wheelhouses, and door impact beams.

A consortium called TWIP4EU with members from steel producers, steel users, research centers, and simulation companies had the goal of developing a simulation framework to accurately model the complex deformation and forming behavior of TWIP steels. The targeted part prototype component was a backrest side member of a front seat, Figure 12. Results were published in 2015.H-58

Figure 12: TWIP4EU Prototype Component formed from TWIP Steel. H-58

Figure 12: TWIP4EU Prototype Component formed from TWIP Steel.H-58

 

In addition to a complex thermomechanical mill processing requirements and high alloying costs, producing TWIP grades is more complex than conventional grades. Contributing to the challenges of TWIP production is that steelmaking practices need to be adjusted to account for the types and amounts of alloying. For example, the typical ferromanganese grade used in the production of other grades has phosphorus levels detrimental to TWIP properties. In addition, high levels of manganese and aluminum may lead to forming MnO and Al2O3 oxides on the surface after annealing, which could influence zinc coating adhesion in a hot dip galvanizing line.D-29

Critical to the performance of TWIP steels is having a microstructure that is fully austenitic.  This is achieved with relatively high carbon (C > 0.5%) and manganese (Mn > 15%). These levels put the alloy at risk for hydrogen embrittlement, otherwise known as hydrogen-induced delayed fracture.  Additions of aluminum were found to be effective in improving the resistance to delayed fracture.  However, the levels of aluminum needed substantially reduced the castability of the molten alloy during continuous casting due to the propensity for aluminum to oxidize, which results in nozzle blockage and slag entrapment.

To reduce the amount of Al and consequently improve the castability of TWIP steels without reducing their resistance to delayed fracture, rare earth (RE) elements can be used.  Rare earth metals react with H2 and form metal hydrides that are much more stable than the ordinary types of hydrogen entrapments in steels.Z-19

During annealing, manganese diffuses to the surface and oxidizes.  The enriched manganese at the surface produces an oxidized layer that reduces the zinc wettability on the steel surface, and limits the ability to achieve a continuous galvanized coating. Solely using a high dew point atmosphere, such as the production strategy with QP steels, is insufficient in these high-Mn TWIP alloys.

A surface treatment process of annealing in a +10°C dew point to promote internal oxidation rather than external oxidation, combined with a subsequent pickling operation to remove any surface manganese oxides, results in a fully austenitic substrate covered by a lean-Mn decarburized ferrite layer, Figure 13. This strategy has led to the commercialization of hot-dip galvanized TWIP steels.P-32 

Figure 13: Cross sectional microstructure of TWIP steel after targeted processing to improve galvanizability.P-32.