This article summarizes a paper entitled, “Weld Quality Study of Projection Nut Welding with Modular Weld Head”, by F. Jiao, et al.F-7

The study investigates the weld quality of projection nut welding with a patent pending “quick release” modular weld head.

The weld nuts used in the study were 3 projection hex-flanged M6 weld nuts. Operating weld currents ranged from 26-32 kA. The welding time was 5 cycles and the applied electrode force was 450 lb. Figure 1 shows the set up for each test. Figure 2 shows the disassembled parts of the quick release modular weld head. Table 1 lists the material properties of the weld faces.

Figure 1:  Projection Nut Welding Set-Up [(a) with regular weld head, (b) with quick-release modular head, and (c) welding parts set up].

Figure 1:  Projection Nut Welding Set-Up [(a) with regular weld head, (b) with quick-release modular head, and (c) welding parts set up].F-7

 

Figure 2:  Disassembled Parts of Patent-Pending Quick-Release Modular Weld Head.

Figure 2:  Disassembled Parts of Patent-Pending Quick-Release Modular Weld Head.F-7

 

Table 1: Material Properties of Weld Faces.

Table 1: Material Properties of Weld Faces.F-7

 

 

Figure 3 shows the cross section images of the projection welds. Both welds made a weld with 100-micron penetration. The weld made with the regular head had a slightly deeper HAZ as indicated by the dashed line. Figure 4 shows the microhardness profile of both projection welds. Generally, the hardness profile of the welds is quite similar.

 

Figure 3:  Optical Microscope Images of the Projection Welds After Etching [(a) with regular head (b) with modular head].

Figure 3:  Optical Microscope Images of the Projection Welds After Etching [(a) with regular head (b) with modular head].F-7

 

Figure 4:  Microhardness of the Projection-Welded Sample with Different Weld Heads.

Figure 4:  Microhardness of the Projection-Welded Sample with Different Weld Heads.F-7

 

 

Figure 5 shows the results of tensile testing on both projection welds. The fracture load with the modular head is higher than that with the regular head at 26 kA. At other currents, the fracture load is very similar.

 

Figure 5:  Variation of Fracture Load with Weld Current for Different Weld Head.

Figure 5:  Variation of Fracture Load with Weld Current for Different Weld Head.F-7

 

 

Figure 6 shows the weld thickness difference between the modular head and the regular head. The results indicate the weld performance of both heads is very similar up to 1000 welds.

 

Figure 6:  Variation of Weld Thickness Difference Between Regular Head and Modular Head.

Figure 6:  Variation of Weld Thickness Difference Between Regular Head and Modular Head.F-7

Related Posts
Filter by
Post Page
homepage-featured-top main-blog Blog Joining Resistance Welding Processes Resistance Spot Welding Arc Welding Automotive Welding Process Comparison resistance welding projection Steel Grades AHSS Joining Dissimilar Materials RSW of Dissimilar Steel RSW Modelling and Performance Tool & Die Professionals Laser Welding High Energy Density Welding
Sort by

Four Steps to Mitigate Liquid Metal Embrittlement When Welding Steel

Liquid Metal Embrittlement (LME) during Resistance Spot Welding (RSW) can cause cracks when welding advanced

18

Resistance Spot Welding with Advanced High-Strength Steels: Cold Stamped and Hot Formed

The discussions relative to cold stamping are applicable to any forming operation occurring at room temperature

18

Steel E-Motive Battery Carrier Frame System and Laser Welded Door Ring Feature Part Integration to Reduce Mass and Cost

The Steel E-Motive concept features an innovative battery housing design and laser welded blank door ring created

18

Resistance Spot Welding AHSS to Magnesium

This blog is a short summary of a published comprehensive research work titled:

18

Resistance Spot Welding: 5T Dissimilar Steel Stack-ups for Automotive Applications

Urbanization and waning interest in vehicle ownership point to new transport opportunities in megacities around the

18

Improvement of Delayed Cracking in Laser Weld of AHSS and 980 3rd Gen AHSS

This article is a summary of the paper entitled, “IMPROVEMENT OF DELAYED CRACKING IN LASER WELD OF AHSS AND

18

Hot cracking investigation in HSS laser welding with multi-scale modelling approach

This article summarizes the findings of a paper entitled, “Hot cracking investigation during laser welding of h

18

Hybrid Laser-Arc Welding (HLAW) Pore Formation and Prevention

This is a summary of a paper by M. Mazar Atabaki, et al, entitled, “Pore formation and its mitigation during

18