In order to improve the microstructure and mechanical properties of Aluminium/Steel resistance spot weld joints, Qiu et al.Q-6 tried a new welding method called resistance element welding (REM), i.e, resistance spot welding with a rivet. In this joining method, a hole was drilled in the overlap area of aluminium alloy sheet and a steel rivet was inserted into the hole. Then resistance spot welding was conducted on the rivet. The schematic of the setup was shown in Figure 1. A 4 µm-thick FeAl IMC layer formed at the rivet/Al interface, while FeAl3 formed at the Aluminium/Steel interface. Maximum tensile shear strength of 3.85 kN and pull-out failure mode can be obtained with a welding current of 21 kA, which was much higher than without a rivet (2.8 kN). Crack propagated along the Aluminium/Steel interface until it was arrested by the rivet. Then the crack propagated along the Al/rivet interface until failure.

 (a) Schematic diagram of resistance spot welding with a rivet; (b) configuration and dimension of the sample (in mm).

Figure 1: (a) Schematic diagram of resistance spot welding with a rivet; (b) configuration and dimension of the sample (in mm).L-9

Recently, Ling et al.L-9 tried resistance element welding of 2-mm-thick 6061-T6 aluminium alloy with a 1.4-mm-thick galvanized DP780 Dual Phase steel with a 5-mm diameter Q235 steel rivet. With optimum welding conditions, the tensile shear strength of resistance element welded Aluminium/Steel can be 7.368 KN with a fracture energy of 18.9 kN, which were 70% and over 6 times higher than those of RSW joints (Figure 2). The fatigue limit of REM joints was 1.8 kN, which was twice those of RSW joints.

Effect of welding current on the tensile shear load of joints.

Figure 2: Effect of welding current on the tensile shear load of joints.L-9

 

Related Posts
Filter by
Post Page
homepage-featured-top main-blog Blog Press Requirements Joining Resistance Welding Processes Resistance Spot Welding Arc Welding Automotive Welding Process Comparison resistance welding projection Mechanical Properties AHSS Steel Grades Joining Dissimilar Materials Citations
Sort by

Four Steps to Mitigate Liquid Metal Embrittlement When Welding Steel

Liquid Metal Embrittlement (LME) during Resistance Spot Welding (RSW) can cause cracks when welding advanced

8

Tensile Testing: Engineering Stress-Strain Curves vs. True Stress-Strain Curves

Tensile testing is one of the most basic formability characterization methods

8

Resistance Spot Welding with Advanced High-Strength Steels: Cold Stamped and Hot Formed

The discussions relative to cold stamping are applicable to any forming operation occurring at room temperature

8

I-4

Citation

8

C-36

Citation

8

Cold Stamped or Hot Formed? Part 1

Equipment, Responsibilities, and Property Development Considerations When Deciding How A Part Gets

8

Current Vehicle Examples

Manufacturers embrace Advanced High Strength Steels as a cost-effective way to satisfy functional and regulatory