Delayed Cracking (Hydrogen Embrittlement)

Delayed cracking caused by hydrogen embrittlement results in decreased toughness, ductility, and load-bearing capacity of a material. It is a concern with some Advanced High-Strength steel (AHSS) grades.

Three triggers must be present for there to be an embrittlement risk:

  1. Use of a susceptible material, such as steel with tensile strength above approximately 1000 MPa and/or the presence of retained austenite in the microstructure,
  2. An environment or processing step where hydrogen is available to diffuse into the steel, and
  3. Presence of a high stress condition, either from forming or during product usage and life cycle.

The interaction between hydrogen and the steel crystallographic structure in the presence of these conditions limits the ability of the steel to deform under load. The steel part will fracture at a lower stress than is anticipated under other conditions. Of particular concern is that fracture may not occur at the time of stamping, since hydrogen can diffuse out of the lattice over time.

High strain areas on parts formed from AHSS are at increased risk for delayed cracking, since the distorted crystallographic lattice allows for an increased hydrogen solubility.  Cut edges are especially troublesome, since the shearing operation work hardens the steel (increasing strength) and damages the microstructure (increasing strain).

AHSS grades that contain retained austenite are also at increased risk for delayed cracking from hydrogen embrittlement. Stamping strains provide the driving force for the TRIP effect, where austenite coverts to martensite. The austenite crystallographic lattice allows for increased hydrogen solubility, so the TRIP effect creates a hydrogen-rich high strength martensite – conditions that promote a greater risk of embrittlement.

Sources of hydrogen include:

  • Breakdown of mill or press applied lubricants,
  • Annealing or heat treating atmospheres, and
  • Electrochemical operations in steel mills or vehicle production such as pickling, electrogalvanizing, welding, phosphate coating, and paint pretreatment, such as e-coating.

Actions to minimize the risk of hydrogen embrittlement includes not over-pickling the surface prior to coating (since pickling uses an acid), heat treating in dew-point controlled atmospheres (below -10 °C or even lower for higher strength grades), and using the e-coating operation as a means to degas the steel.

Global steelmakers take alloying and processing approaches that are specific to their particular infrastructure and equipment. The same grade from two different steelmakers will likely use different alloying approaches. This may lead to different hydrogen embrittlement risks, as well as different tensile property ranges. Use caution when switching suppliers for all AHSS grades.

The procedures to characterize delayed fracture resistance typically involve using a machined sample, pre-strained and placed in an acidic solution for a defined time. SAE J3215S-94 is one such procedure.

Note that cracking in simulative tests does not necessarily indicate that parts made from that material would crack in an automotive environment due to the specific conditions that need to be present for hydrogen embrittlement to occur. When selecting any AHSS, results from simulative tests should be considered in conjunction with the forming and processing history of the steel, the strain state of the formed and processed part, and the operating environment of the part.

Testing & Characterization

Many demands are placed on automotive body structures which influence the material selection process. The impact on safety, manufacturability, and longevity are among the most critical, with each of these balanced against cost and environmental concerns.

Formed sheet metal products experience a complex series of deforming, cutting, and joining before being placed in a body structure, where these components will be subjected to complex loading conditions during the product life cycle. Understanding the failure limits and the conditions which produce failure allows for the design of body structures which can withstand these demands.

Testing helps determine whether a metal is suitable for its intended use. Different tests characterize specific performance aspects. Historically, manufacturers relied on tensile testing to understand metal flow. However, new tests help us understand the behavior of new steel grades and their interactions more thoroughly with new manufacturing technologies.

 

PHS Automotive Applications and Usage

PHS Automotive Applications and Usage

Motivation for PHS usage

In a 2019 study by a global OEM, finite element analysis was used to determine equivalent performance between different thickness and grade combinations in B-pillars and other crash components.O-10  This study found that a 1.6 mm thick hot stamped PHS1500 B-pillar had similar performance as a B-Pillar cold stamped from 3.1 mm thick mild steel, representing a 42% weight savings, Figure 1. Higher strength PHS grades can save an additional 12% to 15% compared to PHS1500. Thus, it may be possible to achieve almost a 50% weight savings by using PHS2000 rather than mild steel in B-pillar applications.

Figure 1: Lightweight potential of several steel grades, compared to mild steel (re-created after Citation O-10)

Figure 1: Lightweight potential of several steel grades, compared to mild steel (re-created after Citation O-10)

 

Weight savings is one reason to choose press hardened steels over cold stamping grades. Although replacing PHS1500 with an 1180 MPa cold formable grade would have a 7% to 8% weight penalty according to the study summarized in Figure 1.O-10  In some cases, this may seem like an acceptable trade-off between weight and process. In recent years, cold forming of 1310 and 1470 (can also be rounded as 1350 and 1500, respectively) MPa steels have been commercially applied in automotive structural parts.K-45  However, press hardening offers several additional advantages over cold stamping of 980 MPa and higher strength grades:B-42

  • The formability of cold stamping higher-strength AHSS steels (even 3rd Gen AHSS) is substantially lower than press hardening steels at elevated temperatures. Their formability typically decreases with increased strength. For example, 3rd Gen 1180 MPa grades may have 16 to 18% total elongation,B-85  whereas a 3rd Gen 1470 MPa grade may have 5 to 6%.K-45 
  • Repeatable dimensional accuracy in cold stamping of 980 MPa and higher strength grades is challenging due to springback and the natural and inherent variations in the mechanical properties of the incoming sheet. Cam-forming and several design countermeasures may be required.K-66
  • Significant wear, chipping, and plastic deformation can be seen in cutting and forming tools, as very high contact pressures may be present.
  • Cold stamping higher-strength AHSS requires high-capacity presses (both in terms of tonnage and energy).
  • Hard-to-predict edge cracks are commonly observed in higher-strength AHSS.

 

Brief History of PHS Usage and Milestones

Press hardenable steel (PHS) production for automotive applications started in 1984. Since this first use through the mid-1990s, door beams were the only press hardened body parts.F-31 Thus, the maximum possible use was limited to 4 parts per car. Depending on a car’s dimensions and the thickness of the sheet, a door beam may weigh between 0.8 kgT-33 to 2.0 kg.M-40 Thus, the total PHS usage at this time was around 3 to 8 kg per car. In a typical mid-size car (D-segment in Europe) the body may weigh around 320 kg without doors and closures, and 420 kg with them.M-41  This results in an estimated usage corresponding to 1% to 2% of the body weight (including doors). By the mid-1990s, several cars had press hardened front and/or rear bumper beams. Thus, the possible maximum usage had been increased to 5 to 6 parts per car.B-43

In 1998, Arcelor patented an aluminium-silicon (Al-Si) coated steel for the press hardening process.L-39 The first automotive application of this coated steel occurred in 2000.V-15  Using coated steel reduces the process cost, since neither the furnace protective atmosphere nor the post-quench sandblasting are requiredV-15, although there is an increase in raw material costs. By 2001, several cars used hot stamped A and/or B-pillars, leading to PHS use in bodies-in-white surpassing 3% for the first time.R-17

In 2002, the first-generation Volvo XC90 had several press hardened and roll form hardened components, making up 6% of the BIW mass. This SUV received 5 stars from EuroNCAP and IIHS frontal and side impact tests.B-44  Ten years after the start of production, the car even achieved a “Good” rating – the highest category – from the very harsh IIHS small overlap test introduced in 2012.I-27

In 2005, Volkswagen rolled out their 6th generation Passat. This car had several components made with a special varnish coating, which facilitated use of a two-step hybrid process in addition to Al-Si coated direct hot stamped components. This car represented the first time press hardening was used on numerous components, including the transmission tunnel and the firewall. For the first time, PHS use in the BIW exceeded 15%.W-31

2008 saw two milestones:

Around the same timeframe, steelmakers started to develop their high energy absorbing PQS grades (see PHS with Higher Elongations).P-21

In 2012, PHS usage surpassed 20% barrier, first with the Volvo V40 (2nd gen. 2012-2019) and then with the Audi A3 (3rd gen. 2012-2020) and VW Golf (7th gen. 2012-2019). The percentage hit 28% with VW Golf.B-45 Figure 2 summarizes this growth.

Figure 2: Summary of PHS evolution: total production in million parts per yearO-11, number of linesH-45, parts per car (approximate) and, BIW percentage (approximate). (Car body CAD data is taken from Citation N-20 and modified for visualization).

Figure 2: Summary of PHS evolution: total production in million parts per yearO-11, number of linesH-45, parts per car (approximate) and, BIW percentage (approximate). (Car body CAD data is taken from Citation N-20 and modified for visualization).

 

Since 2015, many European and North American cars have doubled their PHS usage. In Europe, several VolvoS-81, VW GroupH-43, and FordB-16 models have over 30% of their body (in mass) made of PHS. Some cars may have different PHS usage in different countries. For example, PHS makes up 31% of the body structure in the 6th generation VW Polo in Europe, but in Brazil, this number is reduced to 18.5%.V-16

In 2017, Audi started production of the 4th generation A8. In its earlier generations, A8 was 100% aluminum. The car was mostly aluminum in the third generation (2010-2017). This A8 used a two-layer steel B-pillar, with one layer of cold stamped steel and another layer of press hardened steel. PHS usage was around 3% of the BIW, whereas aluminum usage was over 92%F-32. In the 4th generation A8 on the road since 2017, the body now has 17% press hardened steel.H-44  Several other aluminum intensive cars also have press hardened steels in their bodies for improved crash performance.

In North America, PHS usage has increased rapidly in the last decade. It is not uncommon to see over 10% PHS usage in recently introduced cars. For example, whereas the 9th generation (US Spec) Honda Civic introduced in 2011 had only 1% PHS usage, the 10th generation saw the usage increase to 14%.C-22  The 5th generation Ford Explorer (2012-2019) had only 5% press hardened steelM-42, but exceeds 25% in the 6th generation (2019-present).M-40 The new electric SUV Ford Mustang Mach-E is among the highest PHS-using vehicles in North America in 2020, at 29.5% of its BIW.M-43 The latest generation Chrysler Pacifica has over 11%T-19 and Jeep Wrangler over 18%B-17 of the body (excluding doors and closures) made from press hardened steels. Several GM models have also surpassed 10% barrier, such as Chevrolet Bolt EV with 12%.O-12

In addition, Chinese car makers have begun using significant amount of press hardened steels. According to Ma and others, the first hot stamping line in China was established in 2014.M-74  Figure 3 shows the High-Strength Steel (HSS) usage in Great Wall Motors’ Haval branded SUVs that started production between 2011 and 2017. PHS usage started in the 2014 Haval H2.W-32 The company (Great Wall Motors) invested in an in-house PHS line in 2015.A-64  After the investment, PHS usage exceeded 10%.W-32  In 2018, the total number of hot stamping lines in China was 180. The number increased to 200 in 2020, and by 2022 approached to 260.M-74 The third generation Haval H6 was introduced in mid-2020. The car has over 71% HSS, a hot stamped door ring and one of the first applications of PHS2000 steel.V-12 China is currently the biggest producer and market of “New Energy Vehicles” (plug-in hybrid electric, battery electric or fuel cell). Several electric cars built in China have over 20% PHS. Since 2021, Voyah Free had over 30% PHS in the body in white.W-33 Similarly the more recent Chinese New Energy Vehicles (NEVs) have very high PHS usage, including 2000 and 2200 MPa grades.  These are listed in Table 1.

Figure 3: Increase of PHS usage in Great Wall Motors’ Haval branded SUVs from 2011 to 2017 (re-created after Citation W-32)

Figure 3: Increase of PHS usage in Great Wall Motors’ Haval branded SUVs from 2011 to 2017 (re-created after Citation W-32)

 

The increased use of press hardened steel can be attributed to:

  • Press hardening grades have high global availability, compared to most other cold formable steels over 980 MPa tensile strength.
  • More OEMs and tier suppliers around the globe are investing in the technology. Thus, available capacity for press hardening has increased significantly in the last decade.
  • With the help of commercially available finite element simulation software, more complicated geometries and larger parts can now be designed for press hardening process.

 

Before the First Automotive Application (1973-1984)

Press hardening, as we know it today, was developed in Luleå, Sweden, by Norrbottens Järnverks AB (abbreviated as NJA, translated as Norrbotten Iron Works). The first patent application was completed in 1973, and awarded in 1977.N-23  In 1975, a six-year long industry-university project was initiated at the Luleå University of Technology, together with Volvo Trucks and NJA. Later in 1978 while the project was ongoing, NJA merged with two other steel companies to form Swedish Steel AB (SSAB).B-45

The technology was first commercialized in agriculture components, where the high strength of press hardened steels are favored for wear resistance. In 1981, Norberg Spades and Tool Plant started the first mass production press hardening process. The company produced over 20,000 spades with a cycle time of approximately 20 seconds, while using uncoated 1.5 mm thick sheets.B-45  In 1982, the rights of the patents were transferred to Plannja AB, which was a subsidiary of SSAB. Plannja, a sheet metal forming company, formed Plannja HardTech to specialize in press hardening.

In 1984, automotive application of press hardened steel started with the Saab 9000 side impact door beams, as seen in Figure 4. A total of 4 parts were used in this car.A-66  The uncoated blanks were almost half the thickness of a cold stamped beam.T-26

Figure 4: Door beams of the Saab 9000 (1984-1998): (a) A see-through car in Saab MuseumS-82, (b) the hot stamped door beam part.L-42

Figure 4: Door beams of the Saab 9000 (1984-1998): (a) A see-through car in Saab MuseumS-82, (b) the hot stamped door beam part.L-42 

 

More Automotive Applications (1984-2005)

In 1986, Jaguar XJ (XJ40) also used press hardened door beams.L-43  In 1991, Plannja HardTech received a contract from Ford to supply the door beams of Mondeo, a car to be built and sold both in Europe and North America. The production started in 1993.L-43, B-49  Until December 1994, Plannja HardTech was the sole supplier of press hardened components. By the end of 1994, as the patent rights expired, Accra Teknik AB was established for hot forming of profilesB-46 and Benteler started production of door beams for the VW Polo.L-40

The majority of the press hardened parts were door beams through the mid-1990s, with Plannja HardTech producing approximately 6 million beams in 1996. By this time, the demand for bumper beams was also increasing.F-31  In 1996, the new version of the Renault Safrane included a press hardened bumper beam. The steel was uncoated and supplied by Usinor.B-43  By the end of 1996, EuroNCAP (European New Car Assessment Program) was formed, which increased the pressure on the OEMs for improved crashworthiness.T-26  Plannja HardTech was renamed as SSAB HardTech in 1997. In 1998, both the new Volvo S80L-44 and Ford FocusL-43 were equipped with press hardened bumper beams. SSAB HardTech opened its first plant in North America, in 1998, in Mason, MI.T-26

1998 saw the development of one of the most important breakthroughs in press hardening technology. French steel maker Usinor developed an aluminium-silicon (AS) pre-coated steel, commercialized as Usibor® 1500 (indicating the typical tensile strength, 1500 MPa).C-24, L-39

In 2000, BMW rolled out its new 3 series convertible, the E46 model.  In this vehicle, the A-pillar is made from 3 mm thick uncoated, press hardened sheet. This was the first PHS application at BMW, and one of the first PHS A-pillar reinforcements.S-83, S-84  Accra started delivering roll formed PHS components for the Volvo V70, initially an optional 3rd row seating support. Approximately 10,000 parts/year were supplied.G-28

AS-coated steel was first hot stamped at a French tier 1 supplier, Sofedit.V-15  This grade was first used in the front bumper beam of 2nd Generation Renault Laguna (2000-2007). Laguna 2 was the first car to receive a 5-star safety rating from Euro NCAP.V-10 AS-coated blanks were also used in PSA Group’s Citroën C5 (1st Gen: 2001-2007) in the front bumper beam, and the right/left A-pillars. These three parts weighed a total of 4.5 kg, approximately 1% of the total BIW weight, Figure 5a. About one month later, PSA Group started production of the compact hatchback Peugeot 307. This car had five hot stamped components (right/left A-pillar, right/left B-pillar and rear bumper beam). Unlike the Citroën C5, these parts were uncoated. The total weight was 12 kg, corresponding to 3.4% of the BIW weight.R-17, P-27

Figure 5: Increase in press hardened component usage: (a) 2001 Citroën C5P-27, b) 2002 Volvo XC90L-29 and (c) 2005 VW Passat.H-50

Figure 5: Increase in press hardened component usage: (a) 2001 Citroën C5P-27, b) 2002 Volvo XC90L-29 and (c) 2005 VW Passat.H-50

 

Volvo started producing the XC90 SUV in 2002. The body-in-white with doors and closures weighed 531 kg.B-44  A total of 10 parts, weighing 37 kg are either roll form hardened or direct stamped PHS. This accounts for approximately 7% of the BIW weight.L-43  During its time, this was the highest use of PHS in car body. In Figure 5b, the press hardened components other than the 2nd row seat frame – which is a load bearing body part – are shown.

 

Accelerated Use and Globalization (Since 2005)

The use of press hardened parts increased rapidly after the introduction of the VW Passat in 2005. This car had approximately 19% of its BIW (by weight) made from press hardened steels, Figure 5c. Some parts in this car saw the first use of varnish coated blanks in a two-step hybrid process. Three parts were produced using either an indirect or hybrid process, including the transmission tunnel.H-50 In the same year Ford Mustang (5th Gen: 2005-2014) was rolled out. The car had “form fixture hardened” front and rear bumpers, supplied by Accra.G-28  The bumper geometry and the production method are highlighted in Figure 7 at this link.

In 2006, the Dodge CaliberK-37 and BMW X5P-28 were among the first cars to have tailor-rolled and press hardened components in their bodies. Tailor-rolling is a special process where the thickness of the blank is varied by a flexible rolling process, shown in Figure 6a. The incoming blank is a press hardening steel grade at the thickness equal to or slightly thicker than the targeted thickest portion of the part, and flexibly cold rolled to have a variable thickness distribution. Figure 6b shows the BMW X5 B-pillar.

Figure 6: (a) Tailor Rolling ProcessZ-5, (b) B-pillar of BMW X5 (2nd Gen: 2006-2013).P-28

Figure 6: (a) Tailor Rolling ProcessZ-5, (b) B-pillar of BMW X5 (2nd Gen: 2006-2013).P-28 

 

In 2007, Audi A4 had a tailor welded B-pillar, as shown in Figure 7a.H-32, S-65  In the same year, Volkswagen Tiguan (1st Gen: 2007-2015) became the first car to use a tailored part (also known as tailored tempered part, or multi-strength part) (Figure 7b). The B-pillar was quenched in a die, where the lower portion was heated to create a soft zone.B-20  The Tiguan had 17% of its BIW hot stamped.T-34

Figure 7: B-pillars of: (a) Audi A4, which had a tailor welded blank with HSLA in the lower section, whereas (b) VW Tiguan created a tailored part with a soft zone (re-created after Citations H-32, B-20).

Figure 7: B-pillars of: (a) Audi A4, which had a tailor welded blank with HSLA in the lower section, whereas (b) VW Tiguan created a tailored part with a soft zone (re-created after Citations H-32, B-20).

 

BMW 7 Series (5th Gen: 2008-2015) became the first car to have Zn-coated press hardened components in its body-in-white. The car also contained uncoated parts, as shown in Figure 8. The total PHS usage in this car was approximately 16%.P-20

Figure 8: PHS usage in BMW 7 Series (5th Gen: 2008-2015) (re-created using Citation P-20).

Figure 8: PHS usage in BMW 7 Series (5th Gen: 2008-2015) (re-created using Citation P-20).

 

Since 2010, almost all automakers are using hot stamped steel in their car bodies. In 2012, VW Group unveiled the 3rd generation Audi A3 and 7th generation VW Golf. Both cars were sharing the modular transverse platform (MQB) and had over 24% of their BIW hot stamped. This number was 28% in the 2012 Golf. As of 2020, there are many global cars built on MQB platform (NAFTA, EU, China), and most of them have over 24% hot stamped components.B-14

As the technology advanced, press hardened components found uses beyond lightweighting. One such application reduced the width of the A-pillars to improve the driver’s vision. Some roof bows need to be removed in cars with a panoramic sunroof. In such designs, safety is maintained by reinforcing the A-pillars and cantrails with press hardened steel.N-21

Press hardening allowed car makers to create unconventional cars. In 2011, Hyundai rolled out the 1st generation Veloster. The car was a 3-door coupé (also known as 2+1, with one door on the driver side and 2 doors on the passenger side), and as such contained axisymmetric front doors. Thus, the car could not have a full B-ring, as illustrated in Figure 9a.B-14, R-19 Another unconventional design was the Ford B-Max subcompact MPV sold in Europe between 2012 and 2017. The car had conventional swing doors in the front and two sliding rear doors. The B-pillar was integrated in the doors and was made of press hardened steels. PHS components (integrated B-pillar in front and rear doors, door beams and cantrail) are shown with blue color in Figure 9b.B-14, L-45

Figure 9: Unconventional car designs with PHS: (a) Hyundai Veloster, asymmetric 2+1 doors coupé (re-created after Citation R-19), and (b) Ford B-Max, sub-compact MPV with integrated B-pillars in the doors.L-45

Figure 9: Unconventional car designs with PHS: (a) Hyundai Veloster, asymmetric 2+1 doors coupé (re-created after Citation R-19), and (b) Ford B-Max, sub-compact MPV with integrated B-pillars in the doors.L-45

 

A door ring, as seen in Figure 10, is a single piece that covers the A and B-pillars, hinge pillar, and front portion of the rocker reinforcement. In 2013, the Acura MDX (3rd Gen: 2013-2020) became the first car to have a hot stamped door ring. The part was a tailor welded blank of two sub-blanks, as shown in Figure 10a. The design saved about 6.2 kg weight per car and had high material utilization ratio thanks to sub-blank nesting optimization.A-67, M-46  Currently several Honda (& Acura) and FCA models have hot stamped door rings. One of the most recent applications was in 2017 Chrysler Pacifica with 5 sub-blanks, as shown in Figure 10b. This car also has a PQS550 sub-blank at the lower B-pillar region.D-28

Figure 10: Hot stamped door rings: (a) First application in 2013 Acura MDX had 2 sub-blanks, (b) a more recent application in 2017 Chrysler Pacifica has 5 sub-blanks with PQS550 at the lower B-pillar (re-created after Citations B-14, A-67, D-28)

Figure 10: Hot stamped door rings: (a) First application in 2013 Acura MDX had 2 sub-blanks, (b) a more recent application in 2017 Chrysler Pacifica has 5 sub-blanks with PQS550 at the lower B-pillar (re-created after Citations B-14, A-67, D-28)

 

Since 2013, tubular “hardened steels” are also found in car bodies. One of the first applications was in Mazda Premacy (Mazda 5 in some markets). In this case, a special 3-D hot bending and quenching (3DQ) was employed. The same process was also used in making the A-pillars of the 2nd generation Acura NSX (also known as Honda NSX in some markets, 2016-2022), as seen in Figure 11a.H-29  Since 2018, tubular parts formed with internal pressure — form blow hardened parts — are being used in Ford Focus (4th Generation) and Jeep Wrangler (4th Generation). In the European version of the Ford Focus, a tailor rolled tube with thicknesses between 1.0 and 1.8 mm is used, as depicted in Figure 11b.B-16, B-17

Figure 11: Tubular hardened steel usage in A-pillars of: (a) 2016-2022 Acura NSXH-29, (b) 2018-Present Ford Focus.B-16

Figure 11: Tubular hardened steel usage in A-pillars of: (a) 2016-2022 Acura NSXH-29, (b) 2018-Present Ford Focus.B-16

 

PHS Use in xEVs: Hybrid Electric, Battery Electric, Plug-in

Hybrid Electric, & Fuel Cell Electric Vehicles

The first commercially available Hybrid Electric Vehicle (HEV) was the Toyota Prius (1st Gen: 1997-2003). The second-generation Prius (2003-2009) had very few press hardened components, as shown with red color in Figure 12a. This was the first time Toyota used hot stamped components.M-47 The third generation Prius (2009-2015) had approximately 3% of its BIW press hardened. In the 4th generation Prius released in 2015, the share of >980 MPa steels has risen to 19%.U-10 Figure 12b shows the press hardened parts in the 4th generation Prius.K-38  The 5th generation Prius still has some hot stamped components,T-54 but the body has a number of cold formed 1180 and 1470 MPa gradesF-50, possibly reducing the hot stamped steel usage.

Figure 12: PHS usage in Toyota Prius: (a) 2nd generation (2003-2009) and (b) 4th generation (2015-2022) (re-created after Citations M-47, K-38)

Figure 12: PHS usage in Toyota Prius: (a) 2nd generation (2003-2009) and (b) 4th generation (2015-2022) (re-created after Citations M-47, K-38)

 

Tesla started production of Battery Electric Vehicles (BEV) in 2008, with the Tesla Roadster. This was a low volume vehicle with aluminum and carbon fiber body. Relatively higher volume vehicles, Model S and Model X had aluminum bodies, with PHS reinforcements in the pillars and the bumpers. Model S is known to have a roll-formed PHS bumper beam. High volume Model 3 and Model Y have a significant amount of press hardened components in their bodies.T-35

In 2011, General Motors started production of its first Plug-in Hybrid Electric Vehicle (PHEV), the Chevrolet Volt (known as Opel Ampera in EU and Vauxhall Ampera in the UK). This car had six hot stamped components, including A and B pillars, accounting for slightly over 5% of the BIW mass.P-29

In 2013, Chevrolet modified its supermini car Spark to have a BEV variant. The Spark with internal combustion engine weighed around 1040 kg and had good results from all IIHS tests. In the roof crush test, the car’s upper body was able to carry a total of 4615 kg, approximately 4.4 times of its weight. The EV version, on the other hand, had to carry the weight of the batteries and weighed around 1350 kg. The under body was modified to protect the battery from impacts. The upper body had to be modified to improve the load the roof can withstand in the roof strength test. PHS was used both in upper and underbodies, accounting for 14% of the BIW (Figure 13).H-51

Figure 13: Distribution of different steel families in Chevrolet Spark and Spark EV (re-created after Citation H-51).

Figure 13: Distribution of different steel families in Chevrolet Spark and Spark EV (re-created after Citation H-51).

 

Recent years have seen many BEVs developed and marketed in North America, EU and China markets. Table 1 shows PHS usage in some of these vehicles. For the car bodies listed, only the Nissan Leaf does not have any components made from PHS.T-36  The Jaguar I-PACE, with an aluminum intensive car body, has an innovative PQS-PHS patchwork B-pillarB-21, shown in detail in Figure 12a on the PHS Grades page. Most other BEVs had PHS usage over 10% of their BIW mass by the early 2020s. Renault ZOET-37, Chevrolet BoltO-12 and Opel Corsa-eS-85 are all subcompact cars (B-segment in EU) with steel intensive bodies. Chevrolet Bolt has aluminum doors and closures.O-12 Nissan Leaf and VW ID.3 are compact cars (C-Segment), both have steel intensive bodies. The 1st generation Nissan Leaf had aluminum doors and closuresT-36 and VW ID.3 used extruded aluminum to protect the battery from side impacts [54]. The Audi e-tronE-9, Jaguar I-PACEB-21 and Aiways U5S-86 are medium size SUVs with significant aluminum usage, yet all have some percentage of PHS in their bodies. Polestar 1 is a plug-in hybrid sports car, built-in China and sold under the Volvo Car performance brand, Polestar. The car’s upper body is almost exclusively carbon fiber reinforced polymer (CFRP), whereas the under body is 93% steel, including significant amount of PHS.N-22  ORA R1 is a small city car (A-segment), produced by Great Wall Motors.S-86  The car was the 3rd best-selling EV in China in October 2020.M-48  Voyah, a new brand of Dongfeng Motors, released the iFree SUV.W-33
 

Table 1: PHS usage in several battery electric vehicles (BEVs) around the world. 
Make and Model Production Markets PHS Usage Comments Citation
Nissan
Leaf
2010-2017
(1st generation)
NAFTA, EU
(CN as Venucia e30)

 

0%
  T-36
Renault
ZOE
2012-2024 EU
 
7.5%
BIW (exc. d/c)* T-37
Chevrolet
Bolt
2016-2023
(1st generation)
NAFTA
(EU as Opel Ampera-e)
 
11.8%
  O-12
Opel
Corsa-e
2018-present EU

 
15%

 
19.3%
Underbody
Upperbody (exc. d/c)
S-85
Audi (Q8)
e-Tron
2018-2025 Worldwide
 
27%
BIW (exc. d/c)* E-9
Jaguar
I-PACE
2018-2024 Worldwide
 
3%
Aluminium Intensive Vehicle B-21
Polestar
1
2019-2022 US, some EU, CA, CN
 
18%
  N-22
BMW
iX3
2020-2025
(G08)
Worldwide
 
18%
BIW (exc. d/c)* B-86
Voyah
Free
2021-present CN
 
31%
  W-33
Ford Mustang
Mach-E
2021-present Worldwide
 
30%
BIW (exc. d/c)* M-43
Toyota bZ4x
Subaru Solterra
2022-present Worldwide
 
15%
BIW (exc. d/c)* I-28
VW
ID.Buzz
2022-present Worldwide
 
28%
BIW (exc. d/c)* S-123
Renault Megane
E-Tech
2022-present EU
 
22%
BIW (exc. d/c)* G-55
BMW
i7
2022-present
(G70)
Worldwide
 
24%
BIW (exc. d/c)* B-87
Renault 5
E-Tech
2024-present EU
 
17%
BIW (exc. d/c)* G-56
Volvo
EX90
2024-present Worldwide
 
25%
BIW (exc. d/c)* W-45
Lynk and Co
900
2025-present CN
 
33%
BIW (exc. d/c)* C-43
* BIW (exc. d/c) = Body in White excluding doors and closures

 
 In December 2020, Hyundai announced their new electric platform, E-GMP. The platform will utilize press hardened steel components to secure the batteries.H-52

Another xEV technology is Fuel Cell Electric Vehicle (FCEV), which uses hydrogen as fuel to generate electricity. One of the first FCEV cars was the 2009 Honda FCX Clarity. The car was not sold, but leased in limited numbers. There were less than 50 cars leased in the US.V-18

Since 2015, Toyota has been selling its Mirai FCEV. The car has to carry high pressure hydrogen tanks (2 in the 1st generation and 3 tanks in the 2nd generation), battery, and electric motor. The car is similar in size with Camry, but is about 350 kg (770 lbs) heavier. The first generation Mirai had only B-pillars, cantrails and lateral floor members press hardened.T-38  The second generation has a number of parts with PHS in its under body as well.T-39

The second-generation Honda Clarity FCV was introduced in 2016. This BIW has approximately 15% press hardened components, by weight (including doors and closure weight).K-39  In 2018, Hyundai Nexo became the first fuel-cell car to be tested by EuroNCAP and received 5 stars. The car has A and B pillars, rocker reinforcements, and several under body components made from PHS, as seen in Figure 14.H-53

Figure 14: Press hardened steel usage in Hyundai Nexo Fuel Cell vehicle: (a) side view and (b) top view (re-created after Citation H-53).

Figure 14: Press hardened steel usage in Hyundai Nexo Fuel Cell vehicle: (a) side view and (b) top view (re-created after Citation H-53).

 

Since the early 2020s, electrification has been the main focus of automotive industry. Heavier batteries add at least two segments of weight. To put this in perspective, a subcompact BEV may be as heavy as a mid-size ICE car. Thus the cars had to endure higher roof strength loads as part of federal test requirements (but not part of IIHS), along with requirements associated with various frontal crash conditions. In addition, the severity of EuroNCAP and IIHS side impact tests have increased. EuroNCAP’s side impact energy has been increased by 55%, whereas IIHS’s new side impact test has 82% higher energy compared to the previous tests. EuroNCAP’s new full frontal test also needs higher energy absorbing capability in the front end.B-79

Another big change since 2020 has been using a common upperbody with different underbodies containing different powertrains. Some examples include: BMW X3 (ICE) vs. iX3 (BEV) and Volvo XC40 (ICE) vs. EX40 (BEV). Since BEVs have very high torsional stiffness due to the battery pack, some of the stiffening parts in the upperbody may be removed in the BEV versions.

Before the 2020s, lightweighting was emphasized for the interrelated targets of carbon emission reduction or fuel consumption reduction. With the electrification of the vehicle fleet, the importance of lightweighting now is to enhance the EV range – or payload capacity in commercial vehicles, as seen in next subsection.

In 2024, the Tesla Cybertruck became the first vehicle to have a press hardened double door ring.  The technology quickly became popular in China, with several other cars adopting the technology (see Figures 12 and 13 in PHS Tailored Products). As of 2025, the maximum usage of PHS is still around 38% of the body in white weight. However, there are many cars with over 30% PHS usage, as listed in Table 1 – mostly xEVs.

 

PHS Use in Commercial Vehicles

Press hardening steels improves safety and contributes to lightweighting in passenger vehicles with conventional internal combustion engines and in xEVs. In commercial vehicles, lightweighting can help to increase the payload, as typically these vehicles are limited by their gross vehicle weight (GVW = curb weight + payload). Electrification (HEV, PHEV or BEV) in commercial vehicles further increases the need for press hardened steels in these vehicles.

In Europe, van type commercial vehicles are popular. There are at least 4 distinct classes of panel vans. The smallest ones are typically based on sub-compact (B-segment) car platforms. These cars may be between 3.8 m and 4.2 m long. Vans like Fiat Fiorino and Ford Transit Courier, shown in Figure 15a, can be classified as subcompact. Compact vans are based on C-segment cars and could be sold as commercial or passenger cars. Fiat Doblo (sold as Ram Promaster City, in North America), Ford Transit Connect (shown in Figure 15b), Opel Combo, Peugeot Rifter, Renault Kangoo, VW Caddy are in this segment. These vehicles may have short or long wheelbase (SWB and LWB) versions. Typical lengths are between 4.4 m and 4.5 m in SWB; and between 4.7 m and 4.85 m in LWB. Small vans include Fiat Talento, Ford Transit Custom (shown in Figure 15c), Mercedes Vito/V-Klass, Opel Vivaro/Zafira Life, Peugeot Expert/Traveler, Renault Trafic, and VW Transporter/Caravelle. These cars can be sold as vans or minibuses, with 4.6 m to 5.3 m length options. Lastly, the largest volume and heaviest payload can be carried in full-size vans. Fiat Ducato (Ram ProMaster in North America), Ford Transit, Mercedes Sprinter (Freightliner Sprinter in US), Peugeot Boxer, Renault Master and VW Crafter (shown in Figure 15d) (length data is taken from Wikipedia.org). With new generation commercial vans, over 15% PHS is now also common in Europe.

Figure 15: European panel vans of different sizes: (a) Ford e-Transit Courier (sub-compact)A-89, (b) Ford Transit Connect (Compact)C-25, (c) Ford Transit Custom (Small)B-51, and (d) Volkswagen Crafter (Full-size).V-19

Figure 15: European panel vans of different sizes: (a) Ford e-Transit Courier (sub-compact)A-89A-89, (b) Ford Transit Connect (Compact)C-25, (c) Ford Transit Custom (Small)B-51, and (d) Volkswagen Crafter (Full-size).V-19

 

In North America, pick-up trucks are popular for both commercial and leisure uses. Most OEMs offer pick-up trucks in three different segments: compact, mid-size and full-size. The US Environmental Protection Agency (EPA), on the other hand, classifies trucks as small and standard. Almost all of these pick-up trucks are built as body-on-frame construction with 3 main components: (1) a ladder frame carrying the powertrain and suspension, (2) a cab where the occupants sit and (3) a box which would carry the goods. Honda Ridgeline is one of the exceptions, a standard-size (EPA class) truck with a unibody construction, meaning it does not have a separate frame.B-52

For full-size trucks, the first use of PHS at Ford started with 12th generation F-series in 2009. The largest cab option (commonly called a crew-cab) used a press hardened B-pillar, as shown in Figure 17a. The total weight of PHS components was estimated to be around 8.5 kg, approximately 3% of the total cab weight.M-49  In its 13th generation, Ford switched to an aluminum intensive (92% Al) cab, which did not use PHS in the cab.K-40  However, in the ladder frame of some F-series trucks, additional load transfer parts can be found, as shown in Figure 16c. These parts are produced by the form fixture hardening method. In 2015, trucks without these parts (such as seen in Figure 16a) received a marginal score at IIHS small overlap test. Those with the additional parts (highlighted in Figure 16b) received the “Top Safety Pick” designation.I-19, M-50

Figure 16: Undercarriage view of Ford F-Series: (a) Extended cab, and (b) Crew cab. (c) The tubular parts are made by form fixture hardening process (re-created after Citations I-19, M-50)

Figure 16: Undercarriage view of Ford F-Series: (a) Extended cab, and (b) Crew cab. (c) The tubular parts are made by form fixture hardening process (re-created after Citations I-19, M-50)

 

In 2015, Chevrolet Colorado (and its badge engineered version GMC Canyon) was introduced. This mid-size truck has A and B-pillars hot stamped, accounting for 6% of the cab weight. The truck’s B-pillar reinforcement was a tailor rolled blank with thickness varying between 1.0 and 2.0 mm.M-51  Toyota Tacoma, a direct competitor to Colorado in size, also has press hardened steels in its A and B-pillars.H-54

Figure 17: Hot stamped steel usage in truck cabs: (a) 12th generation Ford F-150 (2009-2015)M-49, (b) 2nd generation Chevrolet Colorado (2011-2024).M-51 *Percentage values are for cab only.

Figure 17: Hot stamped steel usage in truck cabs: (a) 12th generation Ford F-150 (2009-2015)M-49, (b) 2nd generation Chevrolet Colorado (2011-2024).M-51 *Percentage values are for cab only.

 

In 2017, the 2nd generation Honda Ridgeline became the first truck to have a hot stamped door ring, Figure 18a. As opposed to most other pickup trucks, Ridgeline has a unibody design – with no separate frame. Thus, the body and the cab have to be reinforced and weighs about 593 kg. Door rings are tailor welded from 4 sub-blanks, all PHS1500, and weigh approximately 17 kg per side.B-52  In 2018, FCA started production of the 5th generation RAM 1500. This truck also has press hardened door rings, as well as other PHS components in the under and upper body, accounting for almost 15% of the cab and box weight (Figure 18b). These door rings are made from a 6-piece tailor welded blank, with a thickness range between 1.2 and 1.8 mm. A PQS550 sub-blank is used as the lower B-pillar section.R-3

Figure 18: PHS door rings are found in (a) 2017 Honda RidgelineB-52 and (b) 2019 RAM 1500.R-3 *Percentage values include cab and box.

Figure 18: PHS door rings are found in (a) 2017 Honda RidgelineB-52 and (b) 2019 RAM 1500R-3 *Percentage values include cab and box.

 

PHS has also found several uses in heavy commercial trucks. The cab of the 2nd generation Scania truck weighs around 388 kg (including doors). 4% of the cab is made of PHS to pass ECE R29 safety tests. A-pillars have soft zones to further improve toughness of the spot welds.B-53  The Mercedes Actros truck has a roll formed PHS rear bumper, with a rectangular closed profile of 100 x 60 mm and a wall thickness of 3.5 mm. Crossmembers of the frame are also made with the same process.H-55

There are several electric commercial vehicles in production and in development. In Europe, the Mercedes e-Sprinter and VW e-Crafter are commercially available. Ford e-Transit (which will be also sold in NAFTA) is under development. The body is not modified in either the VW e-Crafter nor the Ford e-Transit.V-20, H-56   The battery is attached to the under body with additional elements. Typically, payloads are reduced due to the battery weight. The two battery options offered for the e-Sprinter are one with a long range at the expense of reduced payload and another allowing for increased payload but reduced range.M-52

Rivian developed one of the new generation electric pick-up trucks. Although there has not been an official facelift or a 2nd generation, the BIW has been modified throughout the production of this vehicle. A 2025 presentation has revealed that some aluminum components have been replaced with steel in their so-called 2nd generation body. Press hardened steels have been used in A and B pillars, as well as the hinge pillar, as seen in Figure 19.B-88 

Figure 19: PHS usage in Rivian R1T: (a) first generation, (b) second generation (re-created after Citation B-88.

Figure 19: PHS usage in Rivian R1T: (a) first generation, (b) second generation (re-created after Citation B-88).

 

The Tesla Cybertruck (SOP 2024) has become the first vehicle to introduce a double door ring. This was – at the time of start of production – considered to be the largest single piece hot stamping. The part can be seen in Figure 12 in our article on PHS Tailored Products.

 

Supply

By 2015, hot stamping industry was a 6 billion USD industryV-17 with approximately 100 companies involved.B-14 The industry can be divided into 5 layers:

  1. Raw materials: steel mills, service centers, cold rolling companies (including tailor rolled blanks), blanking companies, laser welded blank companies, and similar.
  2. Tool makers: die makers, die spotting companies, and similar.
  3. Equipment suppliers: press, furnace, automation, cooling system, laser cutting machinery, and similar.
  4. Tier suppliers: Tier 1 or Tier 2 suppliers, typically for automotive OEMs.
  5. OEMs: Original equipment manufacturers, or the vehicle producers themselves.

 

Raw Material Suppliers

SSAB was the first PHS steel producer, and supplied PHS steel to the first Tier 1 PHS stamping company – which was SSAB subsidiary SSAB HardTech AB. Until 1994, HardTech was the only press hardened component supplier and produced approximately 3 to 4 million door beams per year.F-31, T-26  At the time, the estimated total PHS steel supply was on the order of a few thousand tons per year. At the end of 1994, Accra was established as the second Tier 1 supplier.B-46 The company, at least initially, also sourced their steel from SSAB.G-28

Benteler started supplying hot stamped parts to Volkswagen in 1994.L-40 Benteler specified a narrow standard for 22MnB5, commonly known as BTR165 (or sometimes shortened as BTR). In the early 2000s, several OEMs were using this abbreviation for uncoated PHS steels.

By 1996, Usinor (the French steel company which later merged with Spanish steel producer Aceralia and Luxembourg-based Arbed to form Arcelor) is known to supply uncoated PHS grade to Renault.B-43  In 1998, Usinor developed the AS coatingL-39, which would be commercialized in 2000 with the USIBOR 1500® name.V-15

In 2003, the annual European usage of press hardening steel was estimated to be between 60,000 and 80,000 tons.H-46  While the AS-coated steel usage was only 5,000 tons/year in 2006, it increased to 220,000 tons/year by 2009. Five steel mills had the capability to produce AS-coated PHS material in 2009, with three owned by ArcelorMittal, and one each by ThyssenKrupp and Nippon Steel. The latter two companies were running under an ArcelorMittal license.V-15

Earlier projections of future PHS usage have almost always underestimated the growth rate. In 2009, it was projected that in 2013, AS-coated steel usage would be close to 700,000 tons/year.V-15 In reality, nine steel mills produced AS-coated steel in 2013, with the total production exceeding 850,000 tons. In 2013, it was estimated 3 million tons would be achieved by 2020.E-8  Consumption surpassed the 3 million tons threshold in 2018 (Figure 20).B-32

Figure 20: Press hardening steel demand had surpassed the previous estimates.V-15, E-8, B-32

Figure 20: Press hardening steel demand had surpassed the previous estimates.V-15, E-8, B-32

 

Once the steel coils are produced, they are typically sent to steel service centers, where the coils could be slit and/or cut to length. Some service centers may also have blanking lines and laser welding capabilities capable of producing tailored blanks using PHS and/or PQS grades.

In 2014, ArcelorMittal Tailored Blanks (AMTB) had at least three ablation lines for PHS/PQS grades, giving them an annual capacity of producing 3 million tailor welded blanks.E-8  By 2015, the total PHS TWB market was estimated to be 8.4 million blanks. WISCO Tailored Blanks (now known as Baosteel Tailored Blanks) was supplying approximately two thirds of the demand.B-47  By 2019, AMTB had invested in four additional ablation lines.J-20  Estimates of their capacity now exceeds 7 million welded blanks per year.

Tailor rolled blanks (TRB) are mostly supplied by the German company Mubea. An estimated 6,000,000 hot stamped TRB components have been produced per year in 2017. As of 2025, Mubea operates 8 tailor-rolling lines in 3 continents.

 

Tier Suppliers

Currently there are over 700 press hardening lines around the world. Approximately 10% of them are run by OEM’s. A minority of the lines are run for die tryout, R&D and training purposes by steel mills, die makers, tier suppliers, and equipment manufacturers. There are over 60 tier supplier companies, running approximately 75% of the all press hardening lines. Three big tier suppliers are currently operating over 40% of all the lines.  Figure 21 summarizes the press hardened part supply as of 2020.H-45 More recent data is kept confidential.

 
Figure 21: Distribution of press hardening lines in 2020.H-45 (see contact information in Citation B-55 for more up-to-date information information).

Figure 21: Distribution of press hardening lines in 2020.H-45 (see contact information in Citation B-55 for more up-to-date information).

 

In 2003, there were 15 lines in Europe. This number increased to 42 lines in 2009H-46 and over 60 lines by 2012.B-48  According to Billur Metal Form’s Hot Stamping Lines DatabaseH-45, there were over 180 lines in EU27+Turkey in 2020.

The first Tier supplier for press hardened components was HardTech, initially with lines located in Luleå Sweden. The first North American line was also established by HardTech in 1998 in Mason, MI, USA. By 2011, there were already 51 lines in North America.B-48  The number in 2020 was over 130 according to Billur Metal Form’s Hot Stamping Lines Database.H-45

In 2011, over 85 percent of the press hardening lines were in Europe or North America. China, Korea and the rest of the world had only 19 lines.B-48  Only 5 hot stamping lines existed in China in 2010, but the number increased rapidly to 40 by 2015.M-44  By 2020, the total number of lines in China approached 200. South Korea was home to over 40 hot stamping lines in 2020.H-45  A recent study has shown in 2022, China was home to about 260 hot stamping lines.M-74 

Figure 22 is a plot containing parts produced per year (in millions) shown in red and the number of PHS lines globally in blue, showing that they track well at least through approximately 2017. This leads to the conclusion that until that time, the average hot stamping line produced 1 million parts per year. The divergence beginning around 2017 may indicate productivity improvements, since the annual parts produced are outpacing the number of additional lines commissioned. However, since post-2015 production numbers are from an estimate made in 2015, current values may suggest different line productivity trends. Also note that a “double door ring” may be counted as 1 part, when it is actually replacing at least 5 pieces (A-B-C pillars, cantrail, rocker).

Figure 22: Number of hot stamping lines and parts produced per year (literature data from Citations B-48, A-52, H-47, O-11; database information is from Citation H-45)

Figure 22: Number of hot stamping lines and parts produced per year (literature data from Citations B-48, A-52, H-47, O-11; database information is from Citation H-45)

 

Original Equipment Manufacturers

Volkswagen was the first OEM to invest in an in-house press hardening line. By September 2004, there were already 6 press hardening lines within the VW Kassel plant.K-36  The lines were designed to work with the Direct PHS Process, as well as the two-step Hybrid PHS Process. The 6th Generation Passat started production in March 2005. The car had a total of 15 press hardened parts: 12 through the direct process and 3 using the two-step hybrid process, with varnish coatings.W-31 Since 2010, only Al-Si coated blanks have been used with the direct process within Volkswagen. As of 2020, there are a total of 14 press hardening lines at VW: 11 in Kassel and 3 in Wolfsburg. Many current Volkswagen models have over 25% press hardened components in their bodies.

Fiat became the second OEM to invest in press hardening. In 2008, their Cassino plant had five press hardening lines. The lines were accompanied by two trimming presses and eight laser cutting machines.R-18  Fiat models typically have around 5% to 15% of their body components formed using of press hardened steels, as seen in Figure 23.M-45  In 2013, Fiat Group’s Alfa Romeo brand started production of the 4C sport car. In this vehicle, an underbody aerodynamic component was hot formed Al 6016, which also was produced on a press hardening line (not necessarily in-house).C-23

Figure 23: Press hardened component usage in former FCA group (now part of Stellantis) cars between 2006-2018 (re-created after Citation B-14),

Figure 23: Press hardened component usage in former FCA group (now part of Stellantis) cars between 2006-2018 (re-created after Citation B-14),

 

In 2009, BMW became the third OEM to have in-house press hardening lines. Contrary to VW and Fiat, BMW uses zinc-coated blanks formed using the Indirect Process. Their first car to have in-house press hardened components was the BMW 5 GT (F07, 2009-2017).G-38 In the latest generation 5 series (G30, 2016-2023), the PHS usage has surpassed 22% of the body-in-white mass.A-65

As of January 2021, other OEM’s having in-house press hardening lines include (but are not limited to) these companies:

  • Audi: 2 lines in Ingolstadt, since 2009; 2 more lines in Münchsmünster, since 2013.
  • Honda: 1 line in Japan, operating since 2012.
  • SEAT: 3 lines in Martorell.
  • Proton: 1 line in Malaysia, since 2012.
  • Toyota: 1 line in Japan.
  • Volvo: 2 lines in Olofström Sweden, since 2014.
  • Renault: 1 line in Valladolid Spain; 1 more in Douai France, both running since 2014.B-14
  • Ford: 2 lines in China, 2 in Saarlouis, Germany and 3 in Woodhaven, MI, USA.
  • Great Wall Motors: 1 line in Xushui Baoding, China, running since 2015.G-39
  • Opel, 1 line in Kaiserslaitern Germany, started operation on 15 January 2021.L-41

Some OEMs may have access to press hardening lines within their subsidiary tier suppliers. These include Toyota through Toyotetsu and Hyundai through the lines within Hyundai Steel. These are included under “Others” in Figure 21.

 

eren billur, PhD Thanks are given to Eren Billur, Ph.D., Billur MetalForm, who contributed this article.

 

 

Back To Top

 

R-Value

R-Value

R-Value, The Plastic Anisotropy Ratio

The r-value, which is also called the Lankford coefficient or the plastic strain ratio, is the ratio of the true width strain to the true thickness strain at a particular value of length strain, indicated in Equation 1. Strains of 15% to 20% are commonly used for determining the r-value of low carbon sheet steel. Like n-value, the ratio will change depending on the chosen reference strain value.

 

 

Equation 1

 

 

The normal anisotropy ratio (rm) defines the ability of the metal to deform in the thickness direction relative to deformation in the plane of the sheet. rm, also called r-bar (i.e. r average) is the “normal anisotropy parameter” in the formula for Equation 2:

 

Equation 2

 

where r0, r90, and r45 are the r-value determined in 0, 90, and 45 degrees relative to the rolling direction.

For rm values greater than one, the sheet metal resists thinning. Values greater than one improve cup drawing (Figure 1), hole expansion, and other forming modes where metal thinning is detrimental. When For rm values are less than one, thinning becomes the preferential metal flow direction, increasing the risk of failure in drawing operations.

Figure 1: Higher r-value is associated with improved deep drawability.

Figure 1: Higher r-value is associated with improved deep drawability.

 

High-strength steels with tensile strength greater than 450 MPa and hot-rolled steels have rm values close to one. Therefore, conventional HSLA and Advanced High-Strength Steels (AHSS) at similar yield strengths perform equally in forming modes influenced by the rm value. However, r-value for higher strength grades of AHSS (800 MPa or higher) can be lower than one and any performance influenced by r-value would be not as good as HSLA of similar strength. For example, AHSS grades may struggle to form part geometries that require a deep draw, including corners where the steel is under circumferential compression on the binder. This is one of the reasons why higher strength level AHSS grades should have part designs and draw dies developed as “open ended”.

A related parameter is Delta r (∆r), the “planar anisotropy parameter” in the formula shown in Equation 3:

 

Equation 3

 

Delta r is an indicator of the ability of a material to demonstrate a non-earing behavior. A value of 0 is ideal in can making or the deep drawing of cylinders, as this indicates equal metal flow in all directions, eliminating the need to trim ears prior to subsequent processing.

Testing procedures for determining r-value are covered in Citations A-44, I-15, J-14.

 

PHS Automotive Applications and Usage

N-Value

N-Value, The Strain Hardening Exponent

Metals get stronger with deformation through a process known as strain hardening or work hardening, resulting in the characteristic parabolic shape of a stress-strain curve between the yield strength at the start of plastic deformation and the tensile strength.

Work hardening has both advantages and disadvantages. The additional work hardening in areas of greater deformation reduces the formation of localized strain gradients, shown in Figure 1.

Figure 1: Higher n-value reduces strain gradients, allowing for more complex stampings. Lower n-value concentrates strains, leading to early failure.

Figure 1: Higher n-value reduces strain gradients, allowing for more complex stampings. Lower n-value concentrates strains, leading to early failure.

 

Consider a die design where deformation increased in one zone relative to the remainder of the stamping. Without work hardening, this deformation zone would become thinner as the metal stretches to create more surface area. This thinning increases the local surface stress to cause more thinning until the metal reaches its forming limit. With work hardening the reverse occurs. The metal becomes stronger in the higher deformation zone and reduces the tendency for localized thinning. The surface deformation becomes more uniformly distributed.

Although the yield strength, tensile strength, yield/tensile ratio and percent elongation are helpful when assessing sheet metal formability, for most steels it is the n-value along with steel thickness that determines the position of the forming limit curve (FLC) on the forming limit diagram (FLD). The n-value, therefore, is the mechanical property that one should always analyze when global formability concerns exist. That is also why the n-value is one of the key material related inputs used in virtual forming simulations.

Work hardening of sheet steels is commonly determined through the Holloman power law equation:

Holloman LawEquation 1

where
σ is the true flow stress (the strength at the current level of strain),
K is a constant known as the Strength Coefficient, defined as the true strength at a true strain of 1,
ε is the applied strain in true strain units, and
n is the work hardening exponent

Rearranging this equation with some knowledge of advanced algebra shows that n-value is mathematically defined as the slope of the logarithmic true stress – true strain curve. This calculated slope – and therefore the n-value – is affected by the strain range over which it is calculated. Typically, the selected range starts at 10% elongation at the lower end to the lesser of uniform elongation or 20% elongation as the upper end. This approach works well when n-value does not change with deformation, which is the case with mild steels and conventional high strength steels.

Conversely, many Advanced High-Strength Steel (AHSS) grades have n-values that change as a function of applied strain. For example, Figure 2 compares the instantaneous n-value of DP 350/600 and TRIP 350/600 against a conventional HSLA350/450 grade. The DP steel has a higher n-value at lower strain levels, then drops to a range similar to the conventional HSLA grade after about 7% to 8% strain. The actual strain gradient on parts produced from these two steels will be different due to this initial higher work hardening rate of the dual phase steel: higher n-value minimizes strain localization.

Figure 2: Instantaneous n-values versus strain for DP 350/600, TRIP 350/600 and HSLA 350/450 steels.K-1

Figure 2: Instantaneous n-values versus strain for DP 350/600, TRIP 350/600 and HSLA 350/450 steels.K-1

 

As a result of this unique characteristic of certain AHSS grades with respect to n-value, many steel specifications for these grades have two n-value requirements: the conventional minimum n-value determined from 10% strain to the end of uniform elongation, and a second requirement of greater n-value determined using a 4% to 6% strain range.

Plots of n-value against strain define instantaneous n-values, and are helpful in characterizing the stretchability of these newer steels. Work hardening also plays an important role in determining the amount of total stretchability as measured by various deformation limits like Forming Limit Curves.

Higher n-value at lower strains is a characteristic of Dual Phase (DP) steels and TRIP steels. DP steels exhibit the greatest initial work hardening rate at strains below 8%. Whereas DP steels perform well under global formability conditions, TRIP steels offer additional advantages derived from a unique, multiphase microstructure that also adds retained austenite and bainite to the DP microstructure. During deformation, the retained austenite is transformed into martensite which increases strength through the TRIP effect.  This transformation continues with additional deformation as long as there is sufficient retained austenite, allowing TRIP steel to maintain very high n-value of 0.23 to 0.25 throughout the entire deformation process (Figure 2). This characteristic allows for the forming of more complex geometries, potentially at reduced thickness achieving mass reduction. After the part is formed, additional retained austenite remaining in the microstructure can subsequently transform into martensite in the event of a crash, making TRIP steels a good candidate for parts in crush zones on a vehicle.

Necking failure is related to global formability limitations, where the n-value plays an important role in the amount of allowable deformation at failure. Mild steels and conventional higher strength steels, such as HSLA grades, have an n-value which stays relatively constant with deformation. The n-value is strongly related to the yield strength of the conventional steels (Figure 3).

Figure 3: Experimental relationship between n-value and engineering yield stress for a wide range of mild and conventional HSS types and grades.K-2

Figure 3: Experimental relationship between n-value and engineering yield stress for a wide range of mild and conventional HSS types and grades.K-2

 

N-value influences two specific modes of stretch forming:

  1. Increasing n-value suppresses the highly localized deformation found in strain gradients (Figure 1).
    A stress concentration created by character lines, embossments, or other small features can trigger a strain gradient. Usually formed in the plane strain mode, the major (peak) strain can climb rapidly as the thickness of the steel within the gradient becomes thinner. This peak strain can increase more rapidly than the general deformation in the stamping, causing failure early in the press stroke. Prior to failure, the gradient has increased sensitivity to variations in process inputs. The change in peak strains causes variations in elastic stresses, which can cause dimensional variations in the stamping. The corresponding thinning at the gradient site can reduce corrosion life, fatigue life, crash management and stiffness.  As the gradient begins to form, low n-value metal within the gradient undergoes less work hardening, accelerating the peak strain growth within the gradient – leading to early failure. In contrast, higher n-values create greater work hardening, thereby keeping the peak strain low and well below the forming limits. This allows the stamping to reach completion.
  2. The n-value determines the allowable biaxial stretch within the stamping as defined by the forming limit curve (FLC).
    The traditional n-value measurements over the strain range of 10% – 20% would show no difference between the DP 350/600 and HSLA 350/450 steels in Figure 2. The approximately constant n-value plateau extending beyond the 10% strain range provides the terminal or high strain n-value of approximately 0.17. This terminal n-value is a significant input in determining the maximum allowable strain in stretching as defined by the forming limit curve. Experimental FLC curves (Figure 4) for the two steels show this overlap.

    Figure 4: Experimentally determined Forming Limit Curves for mils steel, HSLA 350/450, and DP 350/600, each with a thickness of 1.2mm.K-1

    Figure 4: Experimentally determined Forming Limit Curves for mils steel, HSLA 350/450, and DP 350/600, each with a thickness of 1.2mm.K-1

Whereas the terminal n-value for DP 350/600 and HSLA 350/450 are both around 0.17, the terminal n-value for TRIP 350/600 is approximately 0.23 – which is comparable to values for deep drawing steels (DDS). This is not to say that TRIP steels and DDS grades necessarily have similar Forming Limit Curves. The terminal n-value of TRIP grades depends strongly on the different chemistries and processing routes used by different steelmakers. In addition, the terminal n-value is a function of the strain history of the stamping that influences the transformation of retained austenite to martensite. Since different locations in a stamping follow different strain paths with varying amounts of deformation, the terminal n-value for TRIP steel could vary with both part design and location within the part. The modified microstructures of the AHSS allow different property relationships to tailor each steel type and grade to specific application needs.

Methods to calculate n-value are described in Citations A-43, I-14, J-13.

PHS Automotive Applications and Usage

Necking

Necking: Diffuse Neck and Local Neck

A tensile bar increases in length as it is pulled, with a concurrent reduction in width and thickness. The cross section is rectangular in shape through uniform elongation. After uniform elongation, however, strains concentrate in the reduced section of the tensile test sample, resulting in a non-uniform section of reduced width. This region is known as a diffuse neck. The diffuse neck further accentuates and accelerates the cross-section reduction, leading to a concentration of strains within this region.

A local neck is a narrow band in the sheet metal part that is thinner than its surroundings (Figure 1). This local or through-thickness neck occurs shortly before the traditional fracture of the specimen. When the local neck begins, deformation stops in the remainder of the stamping. In a tensile bar, no deformation occurs along the width of the neck – only increased elongation and thinning. A local neck prevents a deeper section from being formed and serves as a crack initiation site. Additional loading, including fatigue loading during the life of the part, may cause a neck to progress to fracture (Figure 2). The strains resulting in a local neck are defined by the Forming Limit Curve, or FLC

Figure 1:  A local neck prevents forming a deeper section and serves as a crack initiation site.

Figure 1:  A local neck prevents forming a deeper section and serves as a crack initiation site.

             

Figure 2: Necking and fracture on a sample formed with a hemispherical dome.S-57

Figure 2: Necking and fracture on a sample formed with a hemispherical dome.S-57

 

Traditional methods of detecting the onset of necking include tactile or visible sensing of the groove of the neck. Researchers are focusing on the use of non-contact approaches to define a neck. ISO 12004-2 calls for a polynomial fit of data outside the neck, but results from this method are a function of the order of the polynomial as well as the geometry of the tooling and the blank.

Using Digital Image Correlation allows for the detection in curvature evolution in the area that subsequently develops into a neck. The signature is detected for the many types of AHSS grades tested as well as other sheet metals, and correlates well with other methods. Citation S-57 presents an overview of the technique, with greater detail covered in Citations M-19 and S-58. Using the surface data geometry as measured by DIC to detect the true onset of necking enables better and more efficient use of AHSS grades through more reliable knowledge of their actual limits.